Changing the paint is a common response when it peels, but if a thin layer is left on the cleaned surface, the new paint cannot reach the metal either. What actually lies behind it can be oil not fully removed, cleaner left behind, trace silicone, salts left after rinsing, or water left by poor drying, and often two of these at once.

Sometimes a part painted after cleaning lifts with its film at the first pull of tape in inspection, or comes back weeks after shipping with the coating lifting from the edges. The washer ran as usual and the parts looked clean, so the paint or the painting step is the first suspect on the floor. If the peeling goes on after the paint is changed, though, something invisible may still be sitting on the metal.

Peeling turns straight into cost through repainting, scrap and late delivery, and when it shows up after shipping it returns as corrosion in service and as claims. A US Federal Highway Administration report on coating steel starts from the same point: coatings on steel with excessive soluble salts do not reach their expected service life (FHWA, 2014). How long a coating lasts is decided by the surface beneath it as well as by the paint.

Paint has to wet a surface before it can stick. Wetting means a liquid spreads out instead of beading up, and a liquid spreads on a solid when its surface tension is below the solid's critical surface tension (Zisman, 1964). Clean metal has a high critical surface tension, so paint spreads well, but a single layer of a low-energy material such as oil or silicone is enough to stop it spreading. A rough surface adds contact area and helps adhesion (Packham, 2003). Many adhesion failures, however, happen not where paint meets metal but in a thin, easily torn layer trapped between them, known as a weak boundary layer (Bikerman, 1967). Coatings also let water through slowly, so water and salts left at the interface later become the starting point of corrosion and peeling (Grundmeier et al., 2000).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: look at the back of the peeled film and the exposed metal, and wet a freshly cleaned part to see whether the water film breaks (ASTM International, 2021). Those two looks screen several hypotheses at once.

Hypothesis 1: residual oil

Oil is the first thing to suspect. Before cleaning, parts carry machining, rust-preventive or stamping oil, and if it is not all removed, every later step happens on top of it. It shows up on lines where the bath has not been changed for a long time, in tanks with oil floating on top, in cold seasons when the bath struggles to reach temperature, and on days when heavily oiled pressings arrive in bulk. Say a week brings a large run of steel pressings thickly coated in rust preventive, and they go through the washer on the usual settings. The oil layer on the bath grows thicker, and each part passes through it on the way out. If only that week's parts peel in wide patches down to bright metal, this hypothesis is the strong one.

An oil film matters because of surface energy. These oils have low surface energy, so a part covered with them behaves like oil (Zisman, 1964), and paint applied over it sits on oil rather than metal. Oil has little cohesive strength and becomes a weak boundary layer itself (Bikerman, 1967). Aqueous cleaners remove oil in two ways: surfactants break mineral oil into fine droplets dispersed in water, which is emulsifying, and alkali turns animal and vegetable fats into soap, which is saponifying. Both depend on concentration, temperature, time and mechanical action such as spraying or agitation (Durkee, 2006; EPA, 1994). A diluted, cooled or oil-saturated bath therefore removes less, and oil floating on top coats the part again as it is lifted out.

A study comparing waterborne and solventborne epoxy primers on contaminated steel also found that engine oil lowered adhesion, and the primer that did better on clean steel did not consistently keep its lead on contaminated steel (Moshkriz et al., 2026). That is why the surface comes before a change of paint.

Checking starts with the water-break test. Dip a freshly cleaned part in water, lift it out and see whether the film stays continuous; where it breaks or beads, contamination that repels water remains (ASTM International, 2021). For a number, contact angle measurement, which reads the angle a drop makes with the surface, gives surface energy (ASTM International, 2022). Bright, rust-free metal under the peel and a slick back to the film add weight to this hypothesis. On the bath side, log concentration, temperature, the oil layer on top and the time since the last change.

If an oil film is the cause, the bath is where to start. Bring concentration and temperature back into the manufacturer's range, and skim the surface oil or overflow it continuously. Lines with heavy oil loads need a pre-clean stage ahead of the main wash. Surface preparation standards set the same order: scrape off heavy oil first, then clean off the rest (SSPC, 2015). Change the bath by oil load or measurements, not by the calendar, and handle cleaned parts with clean gloves until painting so skin oil does not go back on.

Hypothesis 2: cleaner residue

If paint peels even though the water-break test passed, the cleaner itself comes next. Look for it on lines that run the bath stronger than recommended to clean harder, on equipment with a long transfer between wash and rinse so the solution dries on the part, on lines with a single rinse, and on conversion coating lines that lay down a phosphate or zirconium layer before painting. Picture a hot summer shop where parts leave the washer and ride a conveyor a long way to the rinse tank. On the way, the cleaner dries from the edges and leaves white rims, and the rinse does not take all of them off. If a finger run over a dried part picks up white powder and the film lifts along those marks, look at the cleaner first.

A cleaner can stay on the surface after it has removed the oil. Surfactant molecules have a water-loving end and an oil-loving end, so they cling readily to metal, and builders in alkaline cleaners, such as silicates, phosphates and carbonates, dry into a white powder or thin film (Durkee, 2006). That layer is one more weak boundary layer that keeps paint from touching the metal (Bikerman, 1967).

On conversion coating lines the effect goes a step further. A conversion coating turns the metal surface into a thin phosphate or zirconium-based layer before painting; residual cleaner keeps that layer from growing evenly and carries into the next tank, upsetting its chemistry (Narayanan, 2005). A study on galvanised steel that varied cleaning and rinsing reported that the cleaning method and whether there was a rinse step both affected conversion layer formation and paint adhesion (Baumgartner et al., 2025).

The first things to look for are white stains, water marks and powder that rubs off dried parts. This hypothesis hides from the water-break test, because surfactant left on a surface makes it wet more easily, not less. So when the water film looks normal but paint still peels, check this hypothesis separately. The conductivity and pH of the final rinse show how much cleaner carries over into it; conductivity rises with the salt dissolved in the water. Record the peel with the tape test, in which the film is cut and tape is pressed on and pulled off, so results before and after a change can be compared (ASTM International, 2023).

Cleaner residue calls for work on concentration and rinsing together. First confirm the bath is not stronger than the recommended range; the stronger it runs, the more the rinse has to remove. Shorten the time between wash and rinse so the cleaner does not dry on the part, and split rinsing into two or more stages with clean water in the last. On a conversion coating line, check with both suppliers that the cleaner and the conversion chemistry work together.

Hypothesis 3: trace silicone

This is the hypothesis when scattered round craters appear in the film, or when peeling follows a particular part, mould, operator or bench. Silicone is found in mould release agents, lubricant sprays, some sealants and some gloves and hand creams, so material used outside the paint area can travel in on hands and tools. It deserves a close look in plants where moulding and painting share a building. One day maintenance sprays lubricant on the conveyor hangers, and from the next day craters start to appear on only some parts. The craters cluster near where each part touched its hanger, and other parts from the same wash are fine. This is a scene for reading the spray's data sheet before looking at the bath.

There is a reason silicone causes trouble in such small amounts. This material, polydimethylsiloxane, has very low surface energy, so even a very thin cover makes a spot paint cannot wet (Zisman, 1964). When a low-surface-tension spot forms in a wet film, the surrounding paint is drawn toward higher surface tension and leaves that spot bare as a round crater. A mathematical model describes this flow as driven by the surface tension difference (Evans et al., 2000).

Adhesion falls even where no craters show. In a study of carbon-fibre composite bonded joints contaminated with a silicone release agent, strength fell sharply once silicon passed about 5% of surface atoms, and above 7% little adhesion was left (Markatos et al., 2014). With epoxy primer on steel, a surface contaminated with 1.0 wt% silicone oil gave an adhesion strength, the force needed to pull the film off the surface, of about 2 MPa, far below the roughly 14 to 17 MPa of clean blasted steel (Moshkriz et al., 2026). Silicone does not dissolve in water and resists alkaline cleaning, so it easily survives a wash.

To tell whether it is silicone, look at where the defects gather. The water-break test shows spots the water avoids in a circle (ASTM International, 2021), and contact angle measurement shows low surface energy (ASTM International, 2022). Match the defect sites against moulds, operators, benches and the maintenance schedule, and collect the data sheets of the release agents, lubricant sprays, sealants and hand creams used in the plant, marking those that contain silicone.

With silicone, keeping it out comes before wiping it off. Switch to silicone-free release agents and lubricants in areas painted parts pass through, and control gloves and personal products in the steps before painting. Wipe parts already contaminated with a solvent that dissolves silicone and then clean them, or create a fresh surface by blasting, and recheck with the water-break test. Paint additives that hide craters leave the cause in place and add one more variable, so keep them as a last resort.

Hypothesis 4: residual salts

Look at this hypothesis when parts that were fine just after painting blister weeks or months later and peel as the blisters break. It is likely on lines with short rinses or rinse water left unchanged for long, where hard water goes straight into the final rinse, on parts with many overlaps and recesses the rinse cannot reach, and on products used in humid seasons or where washing and condensation are frequent. Suppose an enclosure shipped in spring, having passed inspection, comes back after the rainy season with small blisters rising from the bottom. Break one and there is moisture inside; scrape back the film and white crystals or rust spots sit beneath. In that case, suspect the last rinse before painting, not the paint.

Blistering starts with osmosis. When rinsing falls short, alkaline salts from the cleaner and calcium, magnesium, chloride and sulfate from hard water stay on the surface. In humid conditions water slowly passes through the film, dissolves those salts at the interface and forms pockets of concentrated salt solution. Osmosis, the pull of water from the dilute side toward the concentrated side, draws in more water, and the pressure pushes the film up into a blister. The weaker the adhesion at the interface, the more easily the blister grows (Cherry, 2011).

Chlorides and sulfates do more than blister: they speed up corrosion under the film (Morcillo, 2003). Once corrosion starts at the interface, adhesion around it fails step by step and the film lifts (Grundmeier et al., 2000). That is why this hypothesis can slip past inspection just after painting and surface only after time in damp conditions.

This hypothesis is confirmed by measuring the salts on the surface directly. The standard method dissolves surface salts into pure water in a small cell stuck to the surface, measures the conductivity of that water and expresses the result as salt per unit area (ISO, 2020). Measuring a cleaned part beside a clean coupon of the same material shows what the rinse leaves behind. On the process side, check final rinse conductivity regularly and watch how much fresh water enters and overflows the rinse tank. Photograph any white crystals or rust spots under the peel as well.

The fix lies in the rinse water. Split rinsing into several stages and feed fresh water into the last stage so it flows back toward the first; this counterflow rinsing gets parts cleaner with the same water (Durkee, 2006). Use pure or deionised water in the last stage, and set a conductivity limit at which the water is changed, matched to the coating specification and the paint maker's requirements. Where rinse water cannot reach, such as recesses and overlaps, change the spray direction or the way the part hangs.

Hypothesis 5: poor drying

The last hypothesis is water. Peeling that starts where water collects, at lower edges, overlaps, welds and around threaded holes, points this way. Typical settings are lines where the dryer after aqueous cleaning is short or runs cool, processes where parts wait a long time between cleaning and painting, and times when the air is damp, as on rainy days, or the parts are cold, as on winter mornings. The first run on a rainy morning is such a scene. Parts leaving the dryer look dry on the outside, but water remains in the overlaps, and in a booth made damp by the rain the margin between the dew point and the part surface temperature narrows. If the same parts painted without trouble on a dry afternoon, water is worth suspecting.

Water left behind does harm in two ways. The first is rust. Water left on steel after aqueous cleaning forms a thin layer of rust within a short time, known as flash rust. Rust is a loosely attached oxide, so paint over it comes off with it. In the same study of epoxy primers on steel, residual corrosion products cut adhesion strength by 70 to 90% (Moshkriz et al., 2026).

The second is trapped water. Water held in overlaps, welds and threaded holes boils out during painting or baking, leaving bubbles and pinholes and trapping water at the interface, where it later becomes the starting point of corrosion and adhesion loss (Grundmeier et al., 2000). Condensation does the same. The dew point is the temperature at which water vapour in the air starts to condense, and a part whose surface falls to the dew point just before painting collects water, while one close to it is at risk. The standard has you work out the dew point from air temperature and relative humidity and compare it with surface temperature (ISO, 2017).

The place to look is where the peel started and what lies beneath it. See whether it began where water collects and whether an even brown rust film sits under it. Pick a few parts at the dryer exit and check their crevices for water, and in the paint booth log air temperature, relative humidity and part surface temperature together to see the margin over the dew point (ISO, 2017). Peeling that clusters on rainy days or on the first run of the morning points to condensation.

Drying problems are fixed right after rinsing. Blow water out of crevices with compressed air, and set dryer temperature and dwell time for the thickest part. If parts wait long between cleaning and painting, agree with the paint maker whether an interim rust preventive is needed. When surface temperature is close to the dew point, delay painting or preheat the parts, following the coating specification and the paint maker for the allowed margin.

Testing the hypotheses

The five hypotheses need not be investigated all at once. Start with what you can see, then what is easy to measure, and rule them out one at a time.

The first step is to see where the film let go. Check, alongside the tape test record, whether it came off the metal or split between coats (ASTM International, 2023). A split between coats points to the painting process before cleaning. If it came off the metal, read the exposed surface. Bright, clean metal points first to oil or cleaner, hypotheses 1 or 2; round craters to silicone, hypothesis 3; blisters and white crystals to salts, hypothesis 4; and an even rust film to drying, hypothesis 5.

Next comes the water-break test. If the water film breaks on a freshly cleaned part, the field narrows to oil or silicone, hypotheses 1 or 3; if it stays even, cleaner, salts and drying, hypotheses 2, 4 and 5, remain (ASTM International, 2021). Then measure bath concentration, temperature and surface oil, and read final rinse conductivity alongside a surface salt test (ISO, 2020). These few measurements screen out much of what is left.

If that still does not settle it, move to a control test. Make panels with only one candidate fixed, paint them side by side with unfixed panels using the same paint under the same conditions, and compare with the tape test (ASTM International, 2023). Match records and patterns too. Checking whether peeling follows a mould, operator, weather, time of day or area of the part separates hypothesis 3, which follows people and tools, from hypothesis 5, which follows weather and time. After the fix, repeat the same test over several runs; it is done only when the peeling does not come back.

One more thing to remember: the hypotheses often overlap. An oil-loaded bath removes less oil and leaves more cleaner, and rinsing those parts longer can then leave them under-dried. In such cases, fix the oil or silicone the water-break test reveals first, then tune rinsing and drying, because problems upstream blur the measurements downstream.

Limits and cautions

Bath concentration and temperature, rinse conductivity limits and the allowed dew point margin differ by product and coating specification, so take the numbers from the cleaner's data sheet, the coating specification and the paint maker. Peeling on plastics, on materials with different surface chemistry such as galvanised steel and aluminium, from powder coating cure conditions, from faulty paint formulation or under-cure, or from excessive film thickness has other causes at work (Baumgartner et al., 2025; Grundmeier et al., 2000). In those cases, and for parts where safety or quality is at stake, do not decide on floor judgement alone; follow standard tests and the paint maker's assessment.

Safety matters too. Alkaline cleaners can harm skin and eyes, and the solvents used to wipe off silicone can be flammable and harmful to breathe. Check the product's safety data sheet, the SDS, before use, and provide gloves, eye protection and ventilation. If peeling recurs across several lines, or does not drop as candidates are changed one by one, send panels and records to the cleaner and paint suppliers or to a laboratory that can analyse surfaces.

Sources

  1. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  2. ASTM International. (2022). ASTM D7490-13(2022), Standard test method for measurement of the surface tension of solid coatings, substrates and pigments using contact angle measurements. https://store.astm.org/d7490-13r22.html
  3. ASTM International. (2023). ASTM D3359, Standard test methods for rating adhesion by tape test. https://webstore.ansi.org/standards/astm/astmd335923
  4. Baumgartner, L., Erbe, A., & Rohwerder, M. (2025). Paint adhesion on titanium and zirconium oxide conversion coated galvanised steel. RSC Applied Interfaces, 2, 1473–1484. https://doi.org/10.1039/D5LF00011D
  5. Bikerman, J. J. (1967). Causes of poor adhesion: Weak boundary layers. Industrial & Engineering Chemistry. American Chemical Society.
  6. Cherry, B. W. (2011). Corrosion and the role of blistering at the coating/substrate interface. Corrosion and Materials, 36(4), 36–41. https://research.monash.edu/en/publications/corrosion-and-the-role-of-blistering-at-the-coatingsubstrate-inte/
  7. Durkee, J. B. (2006). Management of industrial cleaning technology and processes. Elsevier. https://shop.elsevier.com/books/management-of-industrial-cleaning-technology-and-processes/durkee/978-0-08-044888-6
  8. Evans, P. L., Schwartz, L. W., & Roy, R. V. (2000). A mathematical model for crater defect formation in a drying paint layer. Journal of Colloid and Interface Science, 227(1), 191–205. https://doi.org/10.1006/jcis.2000.6877
  9. Federal Highway Administration [FHWA]. (2014). Methodology for analysis of soluble salts from steel substrates (FHWA-HRT-14-026). https://www.fhwa.dot.gov/publications/research/infrastructure/structures/bridge/14026/index.cfm
  10. Grundmeier, G., Schmidt, W., & Stratmann, M. (2000). Corrosion protection by organic coatings: Electrochemical mechanism and novel methods of investigation. Electrochimica Acta, 45, 2515–2533. https://doi.org/10.1016/S0013-4686(00)00348-0
  11. International Organization for Standardization [ISO]. (2017). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application. https://www.iso.org/standard/58061.html
  12. International Organization for Standardization [ISO]. (2020). ISO 8502-9:2020, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 9: Field method for the conductometric determination of water-soluble salts. https://standards.iteh.ai/catalog/standards/iso/ef22ec5a-dd7c-4fc7-a5a2-8d6fbc614aec/iso-8502-9-2020
  13. Markatos, Tserpes, Rau, Brune, & Pantelakis. (2014). Degradation of mode-I fracture toughness of CFRP bonded joints due to release agent and moisture pre-bond contamination. The Journal of Adhesion. https://publica.fraunhofer.de/handle/publica/236002
  14. Morcillo, M. (2003). Soluble salts: Their incidence on the protection of metallic structures by paint coatings. Revista de Metalurgia. https://doi.org/10.3989/revmetalm.2003.v39.iExtra.1123
  15. Moshkriz, A., Ekbrant, B. E. F., & Kiil, S. (2026). Adhesion investigation of waterborne and solventborne epoxy coatings on oil-contaminated and surface-corroded steel substrates. Progress in Organic Coatings, 221, 110534. https://doi.org/10.1016/j.porgcoat.2026.110534
  16. Narayanan, T. S. N. S. (2005). Surface pretreatment by phosphate conversion coatings – A review. Reviews on Advanced Materials Science, 9, 130–177. https://ipme.ru/e-journals/RAMS/no_2905/narayanan.html
  17. Packham, D. E. (2003). Surface energy, surface topography and adhesion. International Journal of Adhesion and Adhesives, 23(6), 437–448. https://doi.org/10.1016/S0143-7496(03)00068-X
  18. Society for Protective Coatings [SSPC]. (2015). SSPC-SP 1, Solvent cleaning. https://codehub.building.govt.nz/resources/sspc-sp-12015
  19. U.S. Environmental Protection Agency [EPA]. (1994). Guide to cleaner technologies: Alternatives to chlorinated solvents for cleaning and degreasing (EPA/625/R-93/016). Office of Research and Development. https://webarchive.library.unt.edu/web/20090512162147/http://www.epa.gov/nrmrl/pubs/625r93016/625r93016.pdf
  20. Zisman, W. A. (1964). Relation of the equilibrium contact angle to liquid and solid constitution. In Contact angle, wettability, and adhesion (Advances in Chemistry, Vol. 43, pp. 1–51). American Chemical Society. https://doi.org/10.1021/ba-1964-0043.ch001

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.