Washing longer or with stronger cleaner is the usual response to spots, but marks also form after the wash, from what the last film of water carries and how it dries. What actually leaves marks can be hard rinse water, cleaner left by poor rinsing, slow drying, oil that settles back or corroded metal, and sometimes two of these at once.

Sometimes parts from the washer dry with white dots scattered over them, or with the whole surface gone hazy. On dark parts and polished faces a ring marks every spot where a droplet sat, and on some parts the marks will not come off with a damp cloth. Longer wash cycles do not help, and the same marks are back the next day.

Spots are more than a cosmetic reject. Washing is usually followed by painting, by conversion coating, which forms a thin protective layer on the metal chemically, by anodising, plating or assembly, and minerals or oil films left on the surface weaken the bond of the next layer. That is why a standard test for such films on metal is used as a check before painting, conversion coating, anodising and plating (ASTM International, 2021). Spots therefore turn into rewashing, rework and coating failure, and unless the cause is found, the same marks return every day.

The basic principle is simple. When water evaporates, what was dissolved in it stays behind on the surface. Minerals in the rinse water, cleaner carried into the rinse and oil floating on the water all belong here. The US Environmental Protection Agency lists water high in total dissolved solids, the sum of solids dissolved in it, as a cause of deposits and staining (EPA, n.d.). How much is left depends on what the last film of water carried, and the shape of the mark depends on how it dries (Deegan et al., 1997). White marks from a reaction of the metal itself form by a different route.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: wipe the mark with a damp cloth, then with dilute vinegar if needed, and look at the surface beneath. If it is smooth and keeps its shine, the mark was a deposit from the water or the cleaner; if it is rough or dull, the metal itself has been attacked.

Hypothesis 1: hard rinse water

On lines that use tap water or groundwater straight for the final rinse, this hypothesis comes first. It is also worth weighing in plants whose water source has changed or whose water varies with the season, and on equipment that dries rinsed parts fast with hot air. A line that rinses parts bound for black paint in groundwater and then dries them with warm air is one such place. On the dark faces of the dried parts, a small white dot sits wherever a droplet was.

The white dots are mostly calcium and magnesium from the water, left behind as solid salts. Their combined amount is called hardness and is usually expressed as mg/L of calcium carbonate. The US Geological Survey classes 0 to 60 mg/L as soft, 61 to 120 as moderately hard, 121 to 180 as hard, and above 180 as very hard (USGS, n.d.). The part of hardness paired with bicarbonate is called temporary hardness. When the water is heated, the bicarbonate breaks down and the calcium settles out as insoluble calcium carbonate, the familiar white scale (DWI, n.d.; WHO, 2011).

The same happens in the droplets left on a part after rinsing. As the water evaporates, the mineral concentration climbs, and once it passes what can stay dissolved, calcium carbonate and other salts are left as solids. Warm parts and hot-air drying speed this up (DWI, n.d.). The result is a white dot wherever a droplet sat, most visible on dark parts, glass and polished faces. The higher the total dissolved solids, the more is left behind (EPA, n.d.).

A drop of dilute vinegar gives a first idea of whether the dots came from the water. If droplet-shaped white dots dissolve or fizz away under the mild acid, a mineral deposit is likely. Next, measure the hardness of the final rinse with test strips or an EDTA titration, the international standard method that adds a reagent bit by bit and reads the sum of calcium and magnesium from a colour change (ISO, 1984). A conductivity meter helps as well. Conductivity rises with dissolved salts, so it shows at once when the water changes with the season or the source. Measure whenever the source changes and whenever spots suddenly increase.

If hardness reads high, switch at least the final rinse to deionised or reverse osmosis water. Reverse osmosis and distillation are recognised ways of cutting dissolved solids (EPA, n.d.). Not every stage needs purified water; what counts is the last water that touches the part. Where purified water is not an option, blow the water off right after rinsing so less is left to evaporate, a step taken up again under hypothesis 3.

Hypothesis 2: cleaner residue

Cleaner residue is likely with washers that have a single rinse tank or rinse water left unchanged for days, on conveyor lines with short rinse times, and on parts with many recesses and holes. Take a washer whose rinse water is changed once at the start of the week. Parts look fine for the first few days, but towards the end of the week they come out evenly hazy, and the area around the holes feels slick to the touch.

What goes into the rinse tank is the wash solution itself. Aqueous cleaners contain surfactants, with one end that holds oil and one that holds water, which lift oil off the part, and builder salts that keep the alkalinity up and hold the calcium in the water. The solution that leaves the wash tank on surfaces and in recesses is called drag-out, and it goes into the rinse (EPA, 1994). With a short rinse, or rinse water left too long, the rinse itself becomes dilute cleaner. When it dries, the salts leave a thin white film and the surfactants a tacky or glossy mark.

Hard water makes this worse. Anionic surfactants that meet calcium ions form an insoluble salt, the precipitate often called lime soap. The calcium level at which a surfactant starts to precipitate is its hardness tolerance, and it depends on the surfactant and on the electrolytes present (Stellner & Scamehorn, 1989). In the wash tank the builders hold the calcium, but in the rinse the cleaner is so dilute that builders fall short. Carried-over surfactant therefore readily meets the calcium in the rinse water and precipitates, leaving a white film that water does not easily remove.

When suspicion falls here, measure rinse tank conductivity at the same time each day and write it down; the rate at which it climbs is the rate at which cleaner builds up. Catching the water that drips from parts after the final rinse and measuring its conductivity shows what is actually left on the surface. A mark that is an even film rather than dots, feels slick or tacky, and is heavier around recesses and holes adds weight to this hypothesis. Check wash tank concentration too, with the supplier's titration method, to confirm it is not running stronger than the recommended range.

The first step is to renew the rinse more often or raise the overflow rate. With two or more rinse tanks, counterflow rinsing, which feeds fresh water into the last tank and lets it flow back to the one before, rinses cleaner with the same water. Letting parts drain over the wash tank for a moment, or adding a spray rinse, cuts drag-out itself (EPA, 1994). If wash concentration is above the recommended range, bring it down, and turn deep-recessed parts on the rack so the solution can run out.

Hypothesis 3: slow drying

Slow drying becomes a problem where parts with threads, deep recesses or overlapping faces are left to air-dry, and where parts still carrying water move straight on to the next step or into stacks. Say threaded brackets are rinsed and then left in their basket to dry at room temperature. Once dry, the lower ends and the roots of the threads hold ring marks that are dark only at the rim.

The ring shape comes from the way a droplet dries. As a droplet dries on a surface, its edge often stays pinned. Evaporation is fastest at the edge, and since the edge cannot move, liquid flows outward from the interior to replace what is lost. That flow carries nearly all the dissolved or suspended material to the edge and leaves a ring once the droplet is dry (Deegan et al., 1997). It is the same principle that makes a coffee spill darkest at its rim, and it occurs across many materials and surfaces as long as the edge stays pinned (Deegan et al., 1997).

A ring needs a pinned edge and a weak counterflow driven by differences in surface tension, called Marangoni flow. When that flow is strong, the material gathers at the centre and dries as a dot (Hu & Larson, 2006). So the same water can leave a ring, a dot or an even film depending on how it dries. What matters on the floor is that the longer a droplet sits, and the more slowly it dries in a recess or between overlapping faces, the more residue collects in one place. Removing the water quickly leaves less water to evaporate and so less residue.

Where the marks gather is the clue. Rings dark only at the rim, or marks clustered where water collects, such as the lower end of a part, recesses, threads and stacked faces, point to drying. Time how long parts take to dry fully in the drying zone, record the drying temperature, and look for parts that move on to the next step or into stacks while still wet. Drying a drop of the same rinse water on a clean glass plate gives a visual comparison of what that water leaves.

Blow the water off right after rinsing. Clearing droplets with compressed air or an air knife leaves less water to evaporate. Rack parts so water runs to a single drip point, and tilt deep-recessed parts. A rinse aid that spreads the water film evenly in the final rinse is another option, and the spotting and filming such products leave are compared by standard methods such as the glassware dishwashing test (ASTM International, 2023). A rinse aid also leaves residue when it dries, though, so keep it within the supplier's recommended range. Raising the drying temperature alone can bring mineral deposits on sooner (DWI, n.d.), so remove the water first and heat second.

Hypothesis 4: redeposited oil

Suspect redeposited oil in a tank that takes in a lot of oil from upstream, has gone a long time without a bath change and has no skimmer. It shows more readily in immersion equipment, where parts come out through the surface. Run a tank that receives oily parts for long enough, and a day comes when water splashed on rinsed parts no longer covers them evenly but splits and beads here and there. Held to the light, those patches show a faint rainbow sheen.

A wash solution removes oil in two ways: it takes the oil into tiny clusters formed by surfactant molecules, or it breaks the oil into small droplets that stay suspended in the water. Oil comes off best when an intermediate phase forms between the oil and the wash solution, and that condition shifts with temperature and surfactant mix (Miller & Raney, 1993). There is a limit, though, to how much oil a wash solution can hold. Once oil builds up and the surfactant is used up, the bath can no longer hold what it has lifted, and the oil rises to the surface.

In that state, parts withdrawn from the tank pass through the floating oil layer and pick oil up again. Rinse water cannot spread over the oil film, so it beads and dries, making the mineral and cleaner marks of hypotheses 1 and 2 heavier. A thin oil film looks iridescent under light and weakens the bond of the next process. A test that checks whether water breaks and beads on a surface is the standard way to detect hard-to-see films that repel water, called hydrophobic films (ASTM International, 2021).

The water-break test checks this hypothesis most directly. Dip a washed part in clean water, lift it out, and see whether the film holds unbroken for a set time (ASTM International, 2021). It gives a pass or fail rather than a number, and it is less sensitive on rough or porous surfaces (ASTM International, 2021). An oil layer or film on the tank surface, together with water that breaks and beads on parts, makes this hypothesis the strong one. The trend in bath oil content can be followed by drawing a fixed sample, letting it stand and seeing how much oil rises.

Remove the surface oil and keep parts from passing through it. Use a skimmer, which picks up floating oil, or an overflow weir; running the bath continuously through an oil-water separator extends its life (EPA, 1994). Before withdrawing parts, push the surface oil aside or add a spray at the exit so the parts avoid the oil layer. If the water-break test fails again and again, change the bath; if a fresh bath saturates quickly, first look for ways to cut the oil coming in from upstream. Oil also lifts poorly when the wash runs below the supplier's recommended temperature, so check that as well (Miller & Raney, 1993).

Hypothesis 5: corroded metal

This hypothesis cannot be left out on lines that wash aluminium or zinc-coated parts in strong alkaline cleaner, or where washed parts are stacked while still wet. All the more so when the marks appear only on aluminium or zinc parts and not on the steel parts from the same line. Stack washed zinc-coated sheets while they are wet, unstack them a few days later, and a white, powdery-looking mark has spread over the faces that touched.

Aluminium suffers in alkali, and zinc in moisture with no air moving. Aluminium is protected by a thin oxide film, but in alkaline solution that film dissolves and reforms over and over while the metal keeps dissolving (Pyun & Moon, 2000). Dissolved aluminium can settle back on the surface as hydroxide when the pH drops in the rinse, leaving white stains or a cloudy film. On zinc-coated parts stacked closely while wet with no airflow, the zinc corrodes quickly and forms a white or grey deposit of zinc oxide and zinc hydroxide (AGA, n.d.). These marks are changed metal rather than deposits from the water, so wiping does not remove them.

If wiping leaves the mark in place, look first at the surface beneath. A rough or dull surface, on aluminium and zinc parts only, points to corrosion. Record wash pH, concentration, temperature and the time parts spend in the solution. For zinc-coated parts, check whether they were stacked wet after washing and whether the marks sit only between the faces that touched (AGA, n.d.). Light white marks may not affect coating life, but medium or heavy marks that have turned black mean much of the zinc layer has been consumed (AGA, n.d.).

Prevention starts with the choice of cleaner. For aluminium and zinc, use a cleaner the supplier states is suitable for that metal, and stay within the supplier's recommended concentration, temperature and contact time. Rinse straight after washing to shorten the time alkali stays on the surface. Stack zinc-coated parts only once fully dry, with spacing so air can move between them (AGA, n.d.). Corrosion marks already formed will not go away under new cleaning conditions, so judge whether the parts are usable against the quality criteria and the coating specification.

Testing the hypotheses

Sorting starts with a wipe. If a damp cloth or dilute vinegar removes the mark and the surface beneath is smooth, it is a deposit, leaving hypotheses 1 to 4; if it stays, or the surface beneath is rough and dull, it is hypothesis 5. White rust on zinc can also dissolve in mild acid, so the state of the surface beneath is a surer sign than whether the mark came off. If marks appear only on aluminium or zinc parts, check hypothesis 5 first.

For a deposit, shape comes next. Droplet dots or rings point to hypotheses 1 and 3, an even film to hypothesis 2, and iridescence or beading to hypothesis 4. If the marks gather only where water collects, hypothesis 3 is at work alongside whichever other one applies.

Measurement then firms up what the shape suggested. High hardness and conductivity in the final rinse point to hypothesis 1; rinse tank conductivity rising day by day points to hypothesis 2. A failed water-break test with oil on the tank surface points to hypothesis 4 (ASTM International, 2021). If timing the drying zone shows parts moving on wet, deal with hypothesis 3 as well.

The control test is to change one thing at a time. Start with the change likely to do most, such as purified water for the final rinse, and compare results on the same parts after each change. Drying one drop of the present rinse water and one of purified water side by side on a glass plate is a simple control too. The final check is that the marks stay away over several runs of the same parts.

When hypotheses overlap, separate those that set how much the water leaves behind, hypotheses 1, 2 and 4, from the one that gathers it into one place, hypothesis 3. Even clean rinse water leaves marks if an oil film makes it bead, and slightly hard rinse water may leave almost nothing if it is blown off at once. Fixing rinse water quality and water removal together is therefore the surer route.

Limits and cautions

Parts with set cleanliness specifications, such as those for painting, plating, medical devices or food contact, are accepted or rejected by the test methods in those specifications. The water-break test gives only a pass or fail, so a figure needs another method such as contact angle measurement (ASTM International, 2021). If the metal has corroded, or marks persist after each hypothesis has been dealt with, take samples to the supplier's technical contact or an analytical laboratory.

Alkaline cleaners can burn skin and eyes. Sodium hydroxide affects the eyes, skin and respiratory system, and contact calls for flushing with water at once (NIOSH, n.d.). Before handling or sampling the solution, read the product's safety data sheet, the SDS, and wear safety glasses and chemical-resistant gloves. When testing a mark with dilute vinegar, never mix it with the cleaner, and rinse the tested spot with water.

Sources

  1. American Galvanizers Association [AGA]. (n.d.). Wet storage stain on galvanized steel: A guide to minimizing and treating wet storage stain. https://galvanizeit.org/uploads/publications/Wet_Storage_Stain_On_Galvanized_Steel.pdf
  2. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  3. ASTM International. (2023). ASTM D3556-23, Standard guide for deposition on glassware during mechanical dishwashing. https://webstore.ansi.org/standards/astm/astmd355623
  4. Deegan, R. D., Bakajin, O., Dupont, T. F., Huber, G., Nagel, S. R., & Witten, T. A. (1997). Capillary flow as the cause of ring stains from dried liquid drops. Nature, 389, 827–829. https://doi.org/10.1038/39827
  5. Drinking Water Inspectorate [DWI]. (n.d.). Water hardness / hard water. UK drinking water regulator. https://www.dwi.gov.uk/consumers/learn-more-about-your-water/water-hardness-hard-water/
  6. Hu, H., & Larson, R. G. (2006). Marangoni effect reverses coffee-ring depositions. Journal of Physical Chemistry B, 110, 7090–7094. https://doi.org/10.1021/jp0609232
  7. International Organization for Standardization [ISO]. (1984). ISO 6059:1984, Water quality: Determination of the sum of calcium and magnesium, EDTA titrimetric method. https://www.iso.org/standard/12258.html
  8. Miller, C. A., & Raney, K. H. (1993). Solubilization-emulsification mechanisms of detergency. Colloids and Surfaces A: Physicochemical and Engineering Aspects, 74(2–3), 169–215. https://doi.org/10.1016/0927-7757(93)80263-E
  9. National Institute for Occupational Safety and Health [NIOSH]. (n.d.). NIOSH pocket guide to chemical hazards: Sodium hydroxide. https://www.cdc.gov/niosh/npg/npgd0565.html
  10. Pyun, S.-I., & Moon, S.-M. (2000). Corrosion mechanism of pure aluminium in aqueous alkaline solution. Journal of Solid State Electrochemistry, 4(5), 267–272. https://doi.org/10.1007/s100080050203
  11. Stellner, K. L., & Scamehorn, J. F. (1989). Hardness tolerance of anionic surfactant solutions. 1. Anionic surfactant with added monovalent electrolyte. Langmuir, 5, 70–77. https://doi.org/10.1021/la00085a014
  12. U.S. Environmental Protection Agency [EPA]. (1994). Guide to cleaner technologies: Cleaning and degreasing process changes (EPA/625/R-93/017). Office of Research and Development. https://webarchive.library.unt.edu/web/20090512162147/http://www.epa.gov/nrmrl/pubs/625r93017/625r93017.pdf
  13. U.S. Environmental Protection Agency [EPA]. (n.d.). Secondary drinking water standards: Guidance for nuisance chemicals. https://www.epa.gov/sdwa/secondary-drinking-water-standards-guidance-nuisance-chemicals
  14. U.S. Geological Survey [USGS]. (n.d.). Hardness of water. Water Science School. https://www.usgs.gov/special-topics/water-science-school/science/hardness-water
  15. World Health Organization [WHO]. (2011). Hardness in drinking-water: Background document for development of WHO guidelines for drinking-water quality. https://www.who.int/teams/environment-climate-change-and-health/water-sanitation-and-health/chemical-hazards-in-drinking-water/hardness

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.