Prepared by
Technical team
Product group
Metalworking Fluids (MWF)

Pouring in more concentrate is the usual response to rusty parts, but it only works when concentration is the cause. What actually brings on rust can be low concentration, microbial growth, salt build-up, spent inhibitor, surfaces that stay wet, or contact with another metal, and often more than one at once.

Sometimes finished parts come out for the next operation with red spots on the surface, and brown stains inside holes or on faces where parts touched. The rust is wiped off and the parts move on, yet a few days later it is back in the same places. It can even keep happening on one sump only, while parts from the machine next to it, running the same fluid, stay clean.

Rust on parts means wiping and rework, scrap, and complaints after delivery. Alongside cooling, lubrication and chip removal, a water-mix fluid has the job of protecting freshly machined parts and the machine from rust (Brinksmeier et al., 2015; OSHA, n.d.). So rust on parts or on the machine counts as one of the signs that a fluid has stopped working (OSHA, n.d.). Whatever lies behind the rust may also be feeding other problems.

Iron in the presence of water and oxygen gives up electrons and oxidises, and the product is rust (Revie & Uhlig, 2008). A water-mix fluid slows this down with inhibitors that cling to the steel as a thin film, and with an alkaline pH that keeps the surface oxide stable (Byers, 2017; Revie & Uhlig, 2008). Rust protection therefore depends on concentration, water quality and the condition of the fluid (HSE, 2021; OSHA, n.d.). Laboratory tests compare protection too. The American standard ASTM D4627 looks for rust marks on cast-iron chips wetted with diluted fluid (ASTM International, 2022), and the German standard DIN 51360-2 rates the rust stain that chips leave on filter paper (DIN, 1981). Chip test results generally relate to how well a fluid protects drilled holes holding chips or stacked parts, but they do not match field conditions in numbers (ASTM International, 2022).

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The first check never changes: draw a sample from the sump where parts rust, measure concentration with a refractometer and pH with a calibrated meter, note the odour, the shape of the rust and when it appeared, and compare the numbers with the manufacturer's recommended range.

Hypothesis 1: low concentration

Concentration tends to fall in sumps topped up with water alone whenever the level drops, in hot weather when evaporation makes top-ups frequent, and on jobs where parts and chips carry out a lot of fluid. It usually drifts down over weeks rather than dropping at once, which makes it easy to miss. A lathe line whose sump has been filled from a hose all summer is such a place. The sump is always full and the fluid looks the same colour, yet one day a thin, even film of rust starts to spread over whole parts.

There is a sequence behind rust from water-only top-up. Every water-mix fluid is designed to run at a set concentration (OSHA, n.d.), and the inhibitor comes in the concentrate. Water evaporates from the sump while concentrate leaves on parts and chips, so topping up with water alone thins the inhibitor by that much. With too little inhibitor the surface film has gaps, and there water and oxygen reach the iron and oxidation starts (Revie & Uhlig, 2008). Low concentration also weakens lubrication and resistance to microbes (HSE, 2021; OSHA, n.d.), so this hypothesis can lay the ground for the ones that follow.

A refractometer is a hand-held tool that reads concentration from how much light bends in the liquid. Measure concentration with it, together with pH, at least weekly, and compare it with the supplier's recommended level (HSE, 2021). Multiply the reading by the manufacturer's correction factor to get the true concentration. If the top-up log shows many water-only additions and the rust is thin and even across whole parts, the case leans towards this hypothesis.

When concentration reads low, top up with fluid premixed at the recommended strength rather than pouring neat concentrate into the sump (HSE, 2021). Logging the date, the reading and the top-up volume shows when the decline began. If the fluid is too strong instead, add water to bring it back into range (OSHA, n.d.). If rust continues once concentration is right, the cause lies elsewhere.

Hypothesis 2: microbial growth

Microbes grow especially well when circulation stops over weekends or holidays, in sumps where a tramp-oil layer blocks oxygen, and where chips and sludge pile up on the bottom (Passman & Küenzi, 2020). A typical scene is the morning after a long holiday: the pump starts and a rotten-egg smell rises from the sump. Parts machined that week start to show rust, and a hand run along the sump wall comes away sticky.

Microbes bring on rust by two routes. Water mixed with organic components makes a good home for bacteria and fungi (Passman & Küenzi, 2020; Saha & Donofrio, 2012). The first route is acid: as microbes break fluid components down for food, they release organic acids that pull pH down (Passman & Küenzi, 2020). On the alkaline side iron's surface oxide is stable and corrosion is slow; as pH falls the film becomes less stable and corrosion speeds up (Revie & Uhlig, 2008). The second route is that the inhibitors themselves are broken down, so rust rises from both sides at once (Passman & Küenzi, 2020; Saha & Donofrio, 2012). Once slime settles on sump walls and pipework, growth returns quickly even after a refill, so cleaning the whole system at each change matters (HSE, 2021; Passman & Küenzi, 2020).

The nose and eyes pick up the signs first. Look for a foul smell, cloudy colour and slime on the sump walls, and check bacteria with dipslides weekly, together with pH (HSE, 2021). A dipslide is a slide coated with growth medium, dipped in the fluid and left for a day or two; the spots that grow show how many bacteria there are. The pH trend over several weeks says more than any single reading, and a steady fall points to microbes first.

If microbes look responsible, take away their food and hiding places first. Skim tramp oil, clear chips, and keep the fluid circulating during stops to shrink the zones without oxygen. If pH has fallen below the recommended range, agree pH correction or biocide addition with the manufacturer, and if bacteria counts are high, clean the system before refilling (HSE, 2021; OSHA, n.d.). Use only the biocide type and dose the manufacturer allows.

Hypothesis 3: salt build-up

Salt builds up where mains or well water is high in salt, in sumps that take a lot of make-up water because of evaporation, and in systems whose fluid has not been changed for a long time. Layouts that let sweat from bare-handed handling, washer solution or heat-treatment residue from earlier steps, or floor-cleaning detergent reach the sump do the same. Take a sump that has run for a long time on top-up alone, never changed. Concentration and pH are both in range, yet pin-point red spots form on the parts, and wiping them off leaves small pits.

Only water leaves the sump by evaporation; the salt stays behind. Each top-up adds a little of the salt in the water, so even when the make-up water looks clean, salt in the fluid climbs over time. Among water constituents, sulfates and chlorides are corrosive to metal and contribute to rust (OSHA, n.d.). Chloride ions attack weak spots in the thin protective film on steel and break it locally, and there a small, deep pit grows, which is pitting corrosion (Frankel, 1998). A study of the water used in wire-cut discharge machining found that even in near-deionised water, small amounts of chloride and sulfate corroded carbon steel severely, and in still water the steel did not reach passivity, the self-protecting oxide state. The inhibitor needed to stop corrosion also rose with sulfate and chloride content (Yashiro et al., 2003). At the same concentration, the fluid faces a stronger attack.

Look at the make-up water first. The basic advice is to check it for hardness, pH and bacteria and to agree suitable water quality with the supplier (HSE, 2021). On top of that, test chloride in the make-up water and the fluid with strips or a laboratory analysis, and see whether the fluid's conductivity climbs with each top-up. Conductivity shows how well the liquid carries electricity, and it rises as more salt dissolves in it. Spot-shaped rust that leaves small pits when wiped adds weight to this hypothesis.

Where the water is high in salt, consider deionised or reverse-osmosis water for dilution. Salt already in the sump does not dilute out with top-ups, so if conductivity and chloride keep rising, set a date for a change. Close the routes by which salt arrives from sweat, washer solution and other processes too, and follow the manufacturer's limits for the product in use.

Hypothesis 4: spent inhibitor

This hypothesis comes up when output rises suddenly, when grinding or cast-iron work with fine chips begins, or when slideway or hydraulic oil leaks from the machine and floats thick on the surface. One example is a line that has just taken on deep-hole drilling in cast-iron housings. The sump readings look no different from usual, but the rust gathers only where chips lay, inside the holes and on faces where stacked parts touch.

Protection can run short even while total concentration is normal. Inhibitors are used up as they cling to freshly cut metal and form a film, so heavy stock removal and fine chips, with their large new surface, can deplete them ahead of the other components. A study of a multicomponent synthetic fluid modelled how fast chip adsorption strips out particular components, and showed they could be replenished before running low (Eppert et al., 2003). Tramp oil leaking from the machine also extracts key components from the fluid (OSHA, n.d.). On top of that, fluid trapped in holes with chips or between stacked parts gets little oxygen, and a narrow gap where oxygen differs from its surroundings is an easy place for local corrosion to start (Revie & Uhlig, 2008). That is exactly the condition iron-chip corrosion tests imitate (ASTM International, 2022; DIN, 1981).

Whether the rust clusters at chips and crevices is the first clue. Set sump fluid and fresh mix at the same concentration side by side on cast-iron chips or filter paper and compare the rust marks; this shows whether the in-use fluid has lost protection (ASTM International, 2022; DIN, 1981). The clearer the sump sample's marks compared with the fresh mix, the further depletion has gone. Note the thickness of the oil layer on the surface as well.

Removing chips and oil comes first. Clear chips from sumps, lines and troughs often (OSHA, n.d.), and shake chips off parts right after machining and drain fluid from holes before stacking. Skim tramp oil, and if the simple test shows weaker protection, ask the manufacturer about a booster additive or plan a change.

Hypothesis 5: parts left wet

Turn to this hypothesis when rust appears not right after machining but hours or a day later. It is likely in humid seasons such as the rainy season, on lines where parts wait long between operations, and where parts are stacked tightly. Picture a line that packs finished parts in layers in a box on a rainy-season evening and sends them to grinding the next morning. The top parts are fine, but the rust grows heavier further down the stack and on faces where parts touch.

Atmospheric corrosion depends heavily on how long a thin film of water stays on the metal, its time of wetness, and ISO 9223, the international standard that classifies atmospheric corrosivity, treats the combination of temperature and humidity as a key factor (ISO, 2012). Early experiments showed that iron rusts much faster once relative humidity passes a critical value (Vernon, 1935). Finished parts carry a thin film of fluid; in humid air it dries slowly, and the little inhibitor in a thin film struggles to last that long. Moving cold parts into warm, humid air makes dew form on them, and that water carries no inhibitor. Water trapped between touching faces cannot evaporate, and inside it oxygen is low and differs from the surroundings, so local corrosion starts easily (Revie & Uhlig, 2008).

Begin by matching timing with the weather. See whether rust clusters while parts wait between operations or on humid days, alongside the plant's temperature and humidity records. Look at airflow and sunlight where parts are kept, and at how they are stacked. Heavy rust on the underside and contact faces of stacks means drying is too slow.

The answer is to dry parts quickly and keep them less wet. Blow parts off after machining and stack them only once dry. If they wait long for the next operation or the season is humid, consider a thin coat of in-process rust preventive. Avoid moving cold parts straight into humid areas, and manage ventilation and dehumidification where parts are stored.

Hypothesis 6: dissimilar metals

This shows up where jigs and supports are made of copper alloy or stainless steel, in shops that machine several materials on one sump, and where chips of different alloys pile up together. Imagine a steel part sitting on a brass support while coolant floods it during machining. Lift the part and rust appears only where the support touched, in the exact shape of the support, while the rest of the surface is clean.

When two different metals touch electrically while immersed together in a liquid that conducts electricity, an electrolyte, they form a small cell. The metal that oxidises more easily becomes the anode and corrodes faster than it would alone; this is galvanic corrosion (ASTM International, 2024; Zhang, 2011). A water-mix fluid with dissolved ions is a good electrolyte. The steel corrodes faster the larger the other metal's area compared with the steel's, and the higher the liquid's conductivity (Zhang, 2011). That is why the salt in hypothesis 3 feeds this hypothesis as well.

Contact corrosion shows in the outline of the rust. See whether it follows the shape of where the part touched a jig, support or other material, with the rest of the part clean. Check which materials share the sump, whether their chips mix, and whether the conductivity measured under hypothesis 3 is high.

When contact is behind it, keeping the metals apart is the most direct fix. Use insulating pads or non-metallic supports where parts meet other metals, keep chips of different materials separate, and hold conductivity down by keeping salt low. If several materials share one fluid, confirm with the manufacturer that the product also protects non-ferrous metals.

Testing the hypotheses

There is no need to investigate all six hypotheses at once. Clear first what a refractometer, a pH meter, the nose and the eyes can answer straight away, and leave the slower tests for later.

Start with concentration, pH and odour. If concentration is low, correct hypothesis 1 first (HSE, 2021); if concentration is right but pH keeps falling and there is odour or slime, treat hypothesis 2 as the main cause (HSE, 2021; Passman & Küenzi, 2020). Only when nothing turns up here is it time to study the rust itself.

The shape and timing of the rust point to the remaining hypotheses. Thin, even rust suggests hypothesis 1; pin-point spots with small pits, hypothesis 3; rust gathered at chips and holes from right after machining, hypothesis 4; rust that appears hours or a day later or clusters on humid days, hypothesis 5; and rust that follows the shape of a jig or support, hypothesis 6. If the rust is spotty, measure chloride in the make-up water and the fluid and the conductivity trend to confirm or rule out hypothesis 3.

The control test is for settling hypothesis 4. Run sump fluid and fresh mix at the same concentration side by side in a chip test; if only the sump sample rusts, the fluid is worn out (ASTM International, 2022; DIN, 1981). If both stay clean but parts still rust, look at drying, storage or contact rather than the fluid. After a fix, measure and log the same items again (HSE, 2021), and close the case only when several checks show the rust has stopped.

Hypotheses can overlap. Microbes may lower pH while water-only top-ups lower concentration too, or built-up salt may raise conductivity and feed contact corrosion as well. When several signs appear together, correct what measurement confirms one at a time, and after each change measure the same items again so the record shows what made the difference (HSE, 2021).

Limits and cautions

Control ranges and test methods differ by product, so take the numbers from the manufacturer's recommendations and the safety data sheet, the SDS, for the product in use. Staining of aluminium or copper alloys, straight oils used without water, and rust after heat treatment or plating have other causes that the hypotheses above do not sort out. Laboratory chip tests are tools for comparing products, or fresh and used fluid, and do not match field performance in numbers (ASTM International, 2022).

Wear protective gloves and eye protection when testing or topping up fluid. Fluid mist is linked to respiratory disease, so NIOSH, the US National Institute for Occupational Safety and Health, sets a recommended exposure limit and advises a comprehensive safety and health programme (NIOSH, 1998). For biocide addition, system cleaning and waste disposal, or rust that keeps returning after these steps, consult the manufacturer or a specialist.

Sources

  1. ASTM International. (2022). ASTM D4627-22, Standard test method for iron chip corrosion for water-miscible metalworking fluids. https://store.astm.org/d4627-22.html
  2. ASTM International. (2024). ASTM G71-81(2024), Standard guide for conducting and evaluating galvanic corrosion tests in electrolytes. https://store.astm.org/g0071-81r24.html
  3. Brinksmeier, E., Meyer, D., Huesmann-Cordes, A. G., & Herrmann, C. (2015). Metalworking fluids: Mechanisms and performance. CIRP Annals, 64(2), 605–628. https://doi.org/10.1016/j.cirp.2015.05.003
  4. Byers, J. P. (Ed.). (2017). Metalworking fluids (3rd ed.). CRC Press. https://www.routledge.com/Metalworking-Fluids/Byers/p/book/9781498722223
  5. Deutsches Institut für Normung [DIN]. (1981). DIN 51360-2, Testing of cooling lubricants; determination of corrosion preventing characteristics of cooling lubricants mixed with water; chip/filter paper method. https://www.din.de/en/getting-involved/standards-committees/nmp/publications/wdc-beuth:din21:909964
  6. Eppert, DeVor, Kapoor, & Rajagopalan. (2003). The effect of chip adsorption on selective depletion from a multicomponent synthetic metalworking fluid. University of Illinois at Urbana-Champaign, IDEALS. https://www.ideals.illinois.edu/items/110202
  7. Frankel, G. S. (1998). Pitting corrosion of metals: A review of the critical factors. Journal of the Electrochemical Society, 145(6), 2186–2198. https://doi.org/10.1149/1.1838615
  8. Health and Safety Executive [HSE]. (2021). MW5, Managing fluid quality: COSHH essentials for machining with metalworking fluids. https://www.hse.gov.uk/pubns/guidance/mw5.pdf
  9. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys: Corrosivity of atmospheres: Classification, determination and estimation. https://www.iso.org/standard/53499.html
  10. National Institute for Occupational Safety and Health [NIOSH]. (1998). Criteria for a recommended standard: Occupational exposure to metalworking fluids (DHHS [NIOSH] Publication No. 98-102). https://www.cdc.gov/niosh/docs/98-102/
  11. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids: Safety and health best practices manual. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids/manual
  12. Passman, F. J., & Küenzi, P. (2020). Microbiology in water-miscible metalworking fluids. Tribology Transactions, 63(6), 1147–1171. https://doi.org/10.1080/10402004.2020.1764684
  13. Revie, R. W., & Uhlig, H. H. (2008). Corrosion and corrosion control: An introduction to corrosion science and engineering (4th ed.). Wiley. https://doi.org/10.1002/9780470277270
  14. Saha, R., & Donofrio, R. S. (2012). The microbiology of metalworking fluids. Applied Microbiology and Biotechnology, 94, 1119–1130. https://doi.org/10.1007/s00253-012-4055-7
  15. Vernon, W. H. J. (1935). A laboratory study of the atmospheric corrosion of metals. Part II: Iron: the primary oxide film. Part III: The secondary product or rust. Transactions of the Faraday Society, 31, 1668–1700. https://doi.org/10.1039/TF9353101668
  16. Yashiro, H., Mocho, M., Yamaguchi, T., Kumagai, N., Iwabuchi, A., Satoh, Y., Nakatsu, T., Kumagai, K., & Kamitaira, T. (2003). Effect of water quality on the corrosion of carbon steel in wire cut discharge machining. Corrosion Engineering, 52(2), 112–115. https://doi.org/10.3323/jcorr1991.52.112
  17. Zhang, X. G. (2011). Galvanic corrosion. In R. W. Revie (Ed.), Uhlig's corrosion handbook (3rd ed.). Wiley. https://search.worldcat.org/title/Uhlig's-corrosion-handbook/oclc/729724608

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.