Rust found after a voyage is easy to blame on seawater getting in, yet moisture in the air inside a closed container can turn to water on the metal by itself. What actually brings the rust can be condensation dripping from the roof, water forming on cold parts, wet wood packaging, salt left on the surface, too little VCI vapour or a faulty oil film, and sometimes two or more at once.

Sometimes a container opens after weeks at sea and parts that left the plant clean are covered in red rust. The packaging looks intact and there is no sign of seawater, yet inside the boxes the top faces carry drip marks or the whole surface has a thin bloom. The same parts never did this on short domestic runs, which makes the cause harder to guess.

Parts that rust in transit are recleaned, re-protected and reinspected at the receiving end, or scrapped. On precision faces and bearing seats even light rust means rework. And if no one settles whether the shipping, the packaging or the rust protection failed, the same damage comes back on the next shipment.

Steel rusts in air through an electrochemical reaction, one in which electrons pass between substances, and it runs only while a thin film of water sits on the surface. In that film iron gives up electrons and dissolves, and oxygen dissolved in the water takes them up (Evans & Taylor, 1972). Experiments in the 1930s already showed that rusting speeds up sharply once relative humidity passes a certain value, the critical humidity (Vernon, 1935). The international standard classifies atmospheric corrosivity by time of wetness, sulfur dioxide and chloride deposition (ISO, 2012), and its earlier edition estimated time of wetness as the hours above 80% relative humidity and above 0 °C (ISO, 1992). When wetting and drying repeat, existing rust takes up electrons like oxygen on rewetting, dissolving more iron and speeding corrosion (Evans & Taylor, 1972). Preventing rust in transit therefore means keeping a water film from forming, or keeping it off the metal when it does.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: photograph the load the moment it is opened, note whether the rust is clustered on top of the load, spread evenly over whole parts, limited to faces touching packaging or sitting at torn spots, and set that against the packing records and the climates at origin and destination.

Hypothesis 1: container rain

Condensation on the container roof builds up in weather with wide day-night temperature swings, in yards where containers stand long in the sun, and during the loading and waiting before and after the voyage. Observations show that temperature and humidity swing more widely and faster during loading, waiting and door opening than on board (Barber, n.d.). This hypothesis fits a scene like this: the doors open, the top boxes are blotchy and wet, and round rust marks are dotted only over the top faces of the parts beneath. Side and bottom faces are clean, and a few boxes near the floor are damp.

The water does not come in from outside; it forms inside. In the sun a container heats up by day, and the warmed air takes up more moisture from the cargo and packaging (Barber, n.d.). At night the steel walls and roof cool first against the outside air, and once their temperature drops below the dew point of the air inside, the temperature at which moisture in the air turns to water, water forms on them (Barber, n.d.; GDV, n.d.). Water on the walls runs down, but water on the roof drips straight onto the cargo. Roof water does not fully dry by day, so it builds up step by step (GDV, n.d.), and this is what is commonly called container rain.

The shape of the rust is the first clue. If rust is clustered as drip marks on the top of the load, the tops of boxes and folds in plastic covers, and the container roof and walls show water marks or rust stains, this hypothesis is the strong one. On the next shipment, send a temperature and humidity logger placed near the top of the load. It records the nightly humidity cycle and the periods when condensation formed.

Stop the falling water first. Cover the top of the load with waterproof sheeting so roof water cannot reach the parts (Imad, 2025), and reduce the moisture in the container itself with desiccant. Size the desiccant by calculation rather than by feel, using a method such as the German standard DIN 55474, which takes in the volume, the humidity and the weight of hygroscopic packaging (Barber, n.d.). Wrap the parts in rust-preventive oil or VCI packaging so any water that gets past the sheeting does not reach bare metal.

Hypothesis 2: cargo sweat

Think of this hypothesis when the seasons or climates at origin and destination differ widely. It tends to appear when a route runs from a cold winter port to a hot, humid region, when parts are heavy castings or thick steel that hold a lot of heat, and when the doors are flung open the moment the container arrives. Imagine thick gearbox housings loaded at a northern port in midwinter and opened at a hot, humid southern port. Soon after the doors open, the surfaces cloud over and feel damp to the touch, and rust spreads evenly, top and bottom alike.

Heavy steel parts hold a lot of heat and warm far more slowly than air. While the part surface stays below the dew point of the surrounding air, water forms on it, and marine insurers call this cargo sweat, defined as condensation that occurs when the cargo is colder than the dew point of the air around it (Gard, 2009). Going the other way, from warm to cold, the steel of the hull or container cools first, and the sweat forms on the steel rather than the parts (Gard, 2009). That is also why ventilation helps only when the outside air has a lower dew point than the air inside (Barber, n.d.; Imad, 2025). Letting in outside air with a higher dew point simply brings more water to the cold parts.

The verdict comes from two values at the moment of opening. Measure the part surface temperature with a surface thermometer, work out the dew point of the surrounding air with a hygrometer, and put the two side by side. If the surface is colder than the dew point, condensation is happening right now. The case firms up if the seasons and temperatures at origin and destination, a record that the parts felt damp right after opening, and worse rust on heavier parts all line up.

The remedy is to wait. Do not open cargo loaded in the cold the moment it arrives; keep the packaging closed until the parts approach the surrounding temperature, then open it. Ventilate by the dew point rule, only when the inside dew point is higher than the outside (Imad, 2025). On routes that cross seasons, consider stepping protection up a level by combining sealed VCI packaging with rust-preventive oil.

Hypothesis 3: wet wood packaging

If the load uses a lot of wooden pallets, crates or corrugated board, suspect the packaging itself. It shows up when packaging was stacked outdoors or under eaves, when loading happened in rain, and when pallets were built from undried green lumber. Picture parts loaded onto pallets that had been stacked beside an outdoor store: on arrival rust has spread from the bottom faces resting on the wooden skids, and mould stains run across the inner walls of the crates.

Steel holds no water, but wood, corrugated board and paperboard are hygroscopic: they take up and give off moisture to match the air around them (Barber, n.d.). When the container warms, water held in these materials passes into the air, and when it cools, that water forms again on the roof and the parts (Barber, n.d.). Pallets of green lumber, with a high moisture content, the share of the wood's weight that is water, give off water in a container, whereas kiln-dried pallets sit near 19% and release none (Barber, n.d.). Heat treatment against pests is not the same as kiln drying, so a heat-treatment mark says nothing certain about moisture content (Barber, n.d.). An insurance-industry handbook concludes that cargo should be loaded as dry as possible to limit container sweat (GDV, n.d.).

When rust started on faces touching wooden skids, crate walls or corrugated board, and the wood shows mould or water stains, it is time to measure the packaging. If pallets and crates from the same lot are still on hand, read their moisture content with a wood moisture meter and log it, and make that reading a step before every loading from now on. Note also where the packaging was stored and whether it rained on the day of loading.

Switch the pallets and crates that carry metal parts to kiln-dried wood, and do not take a heat-treatment mark as proof of drying (Barber, n.d.). Put a moisture-barrier or VCI film between wood and parts so they never touch, and store packaging indoors. Plain plastic wrapped tight traps moist air, and water can form on its inside, so add desiccant or VCI as well. For loads with a lot of wood, never leave the weight of hygroscopic packaging out of the desiccant calculation (Barber, n.d.).

Hypothesis 4: salt residue

Salt stays on the surface when parts are packed or stored near the coast or at a port, when the final rinse after washing leaves salt behind, and when washed parts are handled bare-handed. Picture a shaft lifted from the washer to the oiling bench by someone without gloves. On arrival the rust follows the shape of fingers, and in a few places it has dug in as deep pits.

The trouble with salt lies in how it pulls in water. Salts such as sodium chloride draw moisture from the air once relative humidity passes a set value, the deliquescence humidity, and dissolve into a film of strong brine; for sodium chloride that value is about 75% at room temperature (Schindelholz et al., 2014). Brine carries current easily and chloride ions break the thin protective layer on steel, so rust advances far faster than on a clean surface at the same humidity. Experiments with salt particles on steel found corrosion continuing well below the deliquescence humidity, with water held around the salt crystals named as the cause (Schindelholz & Kelly, 2012; Schindelholz et al., 2014). Salt comes from sea-salt aerosol at ports and on deck, residues from wash water and sweat from bare-hand prints, which is why the standard treats chloride deposition as a separate factor in atmospheric corrosivity (ISO, 2012).

If deep pits, fingerprints or white crystals appear, measure the surface salt. Extract the soluble salts with the Bresle method, ISO 8502-6, in which a water-filled patch is stuck to the surface (ISO, 2020a), and measure the conductivity of that water as a sodium chloride equivalent by ISO 8502-9 (ISO, 2020b). Salt under rust or in crevices may be under-extracted (ISO, 2020a), so a low reading does not clear salt when the pattern fits.

Where salt turns up, start with the washing step. Control the salt content of the final rinse, and wear gloves so no bare hand touches the parts between washing and protection. When packing or storing near the coast, keep parts under cover, and logging surface salt before packing makes the cause easier to find if rust appears next time. Rust can advance under an oil film on a salty surface, so wash the salt off before protection goes on.

Hypothesis 5: too little VCI vapour

Look at this hypothesis when a load packed in VCI bags or film has rusted. It turns up when packs were opened and closed again for an inspection or check en route, when a few small parts went into a large box with a lot of empty space, and when tape or folded openings lifted in transit. A characteristic scene: within one VCI bag the parts lying close against the film are clean, while only those near the lifted tape at the opening or facing a large empty space have rusted. A little water has pooled at the bottom of the bag.

A VCI protects metal through its vapour. A volatile corrosion inhibitor, or VCI, is a temporary protection that slowly vaporises at room temperature, fills a closed space and adsorbs on the metal as a thin protective film (Bastidas et al., 2005; Gangopadhyay & Mahanwar, 2018). How well it works depends on how readily it vaporises, how that changes with temperature, the distance to the metal, and how fast the film forms and breaks down (Bastidas et al., 2005). If a bag is torn or travels open, the vapour escapes and the concentration does not hold, and if the space is too large or the parts sit far from the VCI material, water can form before the film does. Where condensed water pools and parts sit in it, the vapour's protection does not reach them.

The packaging itself is the evidence. See whether the rust clusters at torn bags, seams where tape came loose and packs that were opened and closed again, and whether parts far from the VCI material rusted more within the same pack. Check also for water pooled at the bottom, and whether the manufacturing date and storage time of the VCI material are within the supplier's recommended range. A standard test checks a product's vapour-phase protection on steel specimens in a sealed jar of warm, saturated air, but it is a qualitative test, and compatibility with copper is a separate check (NACE, 2018).

When sealing and placement look to blame, change the packing procedure. Close VCI packaging by folding or heat-sealing as soon as the parts are in, and keep it closed in transit. Follow the supplier's recommended range for the amount and placement of VCI relative to pack volume and part surface area. On routes with heavy condensation, use desiccant together with the VCI, placed so it does not cover the VCI material. For assemblies that mix copper, galvanised steel or aluminium, confirm from supplier data that the VCI suits those metals (NACE, 2018).

Hypothesis 6: faulty oil film

The earlier hypotheses explain where water came from; this one explains why it got through. It shows up on lines that oil parts while they are still wet from machining or washing, where a thin oil meant for short storage is also used for long sea voyages, and where oiled parts are wrapped straight in corrugated board. Take flanges coated with the same oil that never gave trouble on short domestic runs: after a long voyage they arrive rusted from the edges and threads. Wipe the rust off and droplet-shaped stains remain beneath it.

Rust-preventive oil protects the metal in two ways. The oil film keeps water and oxygen from the metal, and the inhibitors in the film attach to the surface and close the remaining gaps. On thin edges, top faces the oil has run off and faces wiped by packaging, the barrier breaks, and when condensation forms, rust starts there. Oil applied over a surface that is still wet traps the water under the film and keeps the surface wet for the whole voyage. On a surface that wets and dries repeatedly, existing rust joins the reduction reaction on rewetting and spreads faster (Evans & Taylor, 1972).

Read the position of the rust together with the oiling records. Check whether rust started on edges, threads and top faces, where films thin out easily, whether droplet-shaped stains sit under it, and whether the film looked cloudy right after oiling. If short domestic shipments with the same oil are fine and only long sea shipments rust, use supplier data and humidity test results to judge whether the oil suits the conditions. A standard test compares oils on steel specimens in a humidity cabinet, but it ranks products against each other and does not stand in for conditions where humidity is not the main cause (ASTM International, 2024).

Dry the parts completely before protection, or use an oil that displaces water. For long sea voyages, choose a film suited to the transit time rather than a thin one meant for short storage, and settle the application method by whether it leaves an even film on edges and threads. Wrap oiled parts in VCI or moisture-barrier film so the packaging does not wipe the film away.

Testing the hypotheses

The six hypotheses do not need six investigations at once. The photographs and rust-position notes taken at opening already screen out several of them. So the first step, before the load is moved, is to record where the rust sits: on top of the load, over whole parts, on faces touching packaging or at torn spots.

The shape of the rust points to a hypothesis. Drip marks clustered on top with water marks on the roof send you first to roof condensation, hypothesis 1 (GDV, n.d.). Even rust over whole parts, top and bottom alike, after a route between very different climates points to cargo sweat, hypothesis 2, so measure part surface temperature and dew point at opening (Gard, 2009). Rust that began where parts touch wood points to hypothesis 3; measure the moisture content of the pallets and crates (Barber, n.d.).

Then turn to why the protection failed. Deep pits, fingerprints or white crystals call for hypothesis 4 and a surface salt measurement (ISO, 2020a, 2020b). Rust clustered at torn or opened packaging points to hypothesis 5; check the sealing and placement of the VCI packs. If no pattern fits and rust began on edges and top faces, move to hypothesis 6 and check the oil type, the film thickness and how dry the parts were before oiling.

Once a judgement forms, confirm it by comparison. Put a temperature and humidity logger in the next shipment, and send packs with only the suspected cause changed alongside packs left as before, then compare them on arrival. Whether the logger shows nightly condensation periods, and whether only the changed packs arrive clean, is the final check.

In practice the hypotheses often overlap. Wet pallets add moisture to the container, the moisture forms on the roof each night and drips down, and the drips start rust at gaps in a thin oil film. In such cases fix one cause on the water side, hypotheses 1 to 3, and one on the protection side, hypotheses 4 to 6, check the effect with a logger, and only then move on to the next.

Limits and cautions

Stainless steel, aluminium, copper alloys, galvanised and painted parts rust differently from ordinary steel and for different reasons, so they need separate treatment, and a flooded container or direct seawater entry is another problem altogether. Critical and deliquescence humidity vary with the type of salt, the surface condition and contaminants, so no single number decides whether a shipment is safe (Schindelholz & Kelly, 2012; Schindelholz et al., 2014).

Before handling rust-preventive oils, VCIs and desiccants, read the product's safety data sheet, the SDS, and wear oil-resistant gloves and safety glasses with oils and solvents. Calcium chloride desiccants turn to brine as they take up water, so keep them away from the parts. For high-value equipment or damage tied to an insurance claim, have a marine surveyor or corrosion specialist investigate, and keep the opened load as found, with photographs and records.

Sources

  1. ASTM International. (2024). ASTM D1748-24, Standard test method for rust protection by metal preservatives in the humidity cabinet. https://store.astm.org/d1748-24.html
  2. Barber, B. (n.d.). Moisture in sea containers: What causes the problems and how to solve them? White paper. Center for Packaging and Unit Load Design, Virginia Tech. Retrieved November 2026. https://unitload.vt.edu/education/white-papers/3-wp-moisture-in-sea-containers.html
  3. Bastidas, D. M., Cano, E., & Mora, E. M. (2005). Volatile corrosion inhibitors: A review. Anti-Corrosion Methods and Materials, 52(2), 71–77. https://doi.org/10.1108/00035590510584771
  4. Evans, U. R., & Taylor, C. A. J. (1972). Mechanism of atmospheric rusting. Corrosion Science, 12, 227–246. https://doi.org/10.1016/S0010-938X(72)90671-3
  5. Gangopadhyay, S., & Mahanwar, P. A. (2018). Recent developments in the volatile corrosion inhibitor (VCI) coatings for metal: A review. Journal of Coatings Technology and Research, 15(4), 789–807. https://doi.org/10.1007/s11998-017-0015-6
  6. Gard. (2009). Don't work up a sweat. Gard News. Gard AS. https://gard.no/insights/dont-work-up-a-sweat/
  7. Gesamtverband der Deutschen Versicherungswirtschaft [GDV]. (n.d.). Formation of container sweat in radiation weather. Container handbook, 10.3.5.1. Online edition, retrieved November 2026. https://containerhandbuch.de/chb_e/scha/scha_10_03_05_01.html
  8. Imad, T. (2025). The problem of sweat. Risk Alert, 113. Steamship Mutual. https://www.steamshipmutual.com/publications/articles/problem-sweat
  9. International Organization for Standardization [ISO]. (1992). ISO 9223:1992, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification. Superseded edition. https://cdn.standards.iteh.ai/samples/16855/c18be4081cfc44aba101e3448e3539b6/ISO-9223-1992.pdf
  10. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  11. International Organization for Standardization [ISO]. (2020a). ISO 8502-6:2020, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 6: Extraction of water soluble contaminants for analysis, Bresle method. https://webstore.ansi.org/preview-pages/ISO/preview_ISO+8502-6-2020.pdf
  12. International Organization for Standardization [ISO]. (2020b). ISO 8502-9:2020, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 9: Field method for the conductometric determination of water-soluble salts. https://www.iso.org/standard/73862.html
  13. NACE International [NACE]. (2018). NACE TM0208-2018, Laboratory test to evaluate the vapor-inhibiting ability of volatile corrosion inhibitor materials for temporary protection of ferrous metal surfaces. Now AMPP. https://webstore.ansi.org/standards/nace/nacetm02082018
  14. Schindelholz, E., & Kelly, R. G. (2012). Wetting phenomena and time of wetness in atmospheric corrosion: A review. Corrosion Reviews, 30, 135–170.
  15. Schindelholz, E., Risteen, B. E., & Kelly, R. G. (2014). Effect of relative humidity on corrosion of steel under sea salt aerosol proxies. Journal of The Electrochemical Society, 161(10), C450–C459. https://doi.org/10.1149/2.0221410jes
  16. Vernon, W. H. J. (1935). A laboratory study of the atmospheric corrosion of metals. Part II.–Iron: The primary oxide film. Part III.–The secondary product or rust. Transactions of the Faraday Society, 31, 1668–1700. https://doi.org/10.1039/TF9353101668

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.