KALTEC

BlogApplication notes

Why did parts rust in storage?

Type
Application notes
Published
20 November 2026
Prepared by
Technical team
Product group
Corrosion Prevention

When stored parts rust, the usual move is to blame the rust preventive and change products, but rust follows not only a weak film but also stronger conditions for water to form on the metal. What actually brings it can be humid storage air, dew on cold parts, a weak film, residue under the film, or damp, acidic packaging, and a source of water can meet a weak film at the same time.

Sometimes parts that were machined, inspected, coated with rust preventive and shelved are taken out a few weeks later for shipping with a light bloom of rust over them. Some boxes are fine while others have red spots on every edge, and people point out that the same preventive never did this before this year. Changing the preventive is tempting, but first it has to be settled whether the cause lies in the film or in the store.

Rust in storage is costly because it lands on parts that have already been machined and inspected. Even light rust means cleaning and re-preserving, and rust on precision faces or threads spoils dimensions and fits, so parts get scrapped. Found in a customer's warehouse after shipping, it comes back as a quality claim.

Rusting of iron is an electrochemical reaction. Inside a water film on the surface, iron gives up electrons and dissolves, acting as the anode, while oxygen dissolved in the same film takes those electrons, acting as the cathode. The dissolved iron meets oxygen and water and turns into red rust by way of iron hydroxides (Leygraf et al., 2016; Revie & Uhlig, 2008), and without a water film the ions have no path and the reaction nearly stops. The international standard likewise treats atmospheric corrosion as set by time of wetness, the time a thin water film is present, together with pollutants (ISO, 2012). A rust preventive is a temporary barrier that keeps that water film and oxygen off the metal; common forms are inhibitors dissolved in a solvent that leave a thin film once it evaporates, oils, and volatile corrosion inhibitors, or VCIs, that spread as vapour through a closed space (DoD, 1993; Gangopadhyay & Mahanwar, 2018). For any of them, the outcome makes sense only when how long the film holds is weighed against how strong the conditions for water are.

When this happens, the technical team sets up the five hypotheses below and strikes them off one by one. The first check is the same every time: photograph where the rust is and what it looks like, sort it into even and light, concentrated on top faces and edges, shaped like fingerprints or water marks, or where packaging touched, and write the storage time and the product's recommended protection period beside it.

Hypothesis 1: humid storage air

Rust from humidity depends on the season and the spot. It is worse in the rainy season, in unventilated corners and on shelves near the floor, and it forms light and even over whole parts, or over many parts on the same shelf, rather than on one patch. After a long, wet summer, for instance, boxes on the bottom shelf in a back corner open to parts tinged evenly orange all over, while the same parts on a shelf by the entrance are clean.

Rust can start with no visible water at all. Water vapour in the air always clings to a metal surface a few molecules thick, and at low humidity this water is too thin for ions to move. As relative humidity rises, the layer thickens into a path ions can travel through, an electrolyte (Leygraf et al., 2016; Schindelholz & Kelly, 2012), and this threshold is called the critical relative humidity. In classic experiments rusting of iron sped up sharply above it, and the jump was far larger in air carrying pollutants such as sulfur dioxide (Vernon, 1935). The threshold should be read not as one number but as a range that shifts with surface condition and contamination (Leygraf et al., 2016; Vernon, 1935).

When the water film is very thin, oxygen has only a short way to travel to the metal, so the cathodic reaction can run faster under a thin film than under immersion (Stratmann & Streckel, 1990a, 1990b). Once formed, the porous rust layer holds water, so that spot stays wet longer even after humidity falls, and rust keeps growing where it first appeared (Leygraf et al., 2016; Vernon, 1935).

Look at duration, not the average. Put a temperature and humidity logger in the storage area and record hourly relative humidity for at least a few weeks, and it shows how long each day, and for how many days running, humidity stays high. A logger on a shelf with even rust and another on a clean shelf, compared side by side, show the difference between spots as well.

If high humidity runs on for long stretches, the thing to fix is the air rather than the film: dehumidify, ventilate and keep stock off the floor. Where the air cannot be changed, move to a longer-lasting film type for the storage period and setting, or add sealed packaging. Compare candidate products under the same humidity test (ASTM International, 2024).

Hypothesis 2: dew on cold parts

In winter and at the turn of the seasons, near doors where outside air comes and goes, and when cooled parts are packed straight away, condensation is what brings the rust. Its position differs too: it follows top faces, hollows where water pools and run marks downwards, mixed with spotty rust shaped like droplets. A pallet of parts left overnight beside a draughty loading-bay door, then checked after the door goes up in the morning and warm, humid air rolls in, looks like this. The surfaces are covered in fine droplets, and a few days later each spot carries a rust mark.

How much water vapour air can hold is set by temperature. When air cools below its dew point, the temperature at which vapour starts turning to water, the excess vapour becomes droplets. Metal parts are heavy and warm slowly, so when parts chilled overnight meet warm, humid morning air, the air warms but the part surface stays below the dew point, and dew forms (ISO, 2017; Leygraf et al., 2016). The international standard for painting likewise judges condensation risk by the gap between surface temperature and dew point (ISO, 2017).

Condensation is worse than humid air for two reasons: it delivers far more water to the surface, and it cycles between wet and dry. While wet, existing rust takes electrons from the iron in place of oxygen and keeps the reaction going; once dry, oxygen in the air turns it back into rust. As the cycle repeats, rust can build faster than under constant wetness (Evans, 1965). Droplets on a preventive film work into its weak spots, and films with little water-displacing ability do not last long (DoD, 1993).

Measure dew point and part temperature at the same moment. Work out the dew point from air temperature and humidity, measure part temperature with a surface thermometer alongside, and look for the periods when the part is near or below the dew point (ISO, 2017). Measuring separately near the doors and deep inside the store, and on freshly cooled and room-temperature parts, shows which places and times carry the risk.

The way to less condensation is a smaller temperature gap. If parts dip below the dew point at times, reduce temperature swings in the store and keep stock away from areas where outside air enters. Let cold parts reach room temperature before packing, and choose a water-displacing film type where condensation is frequent (DoD, 1993).

Hypothesis 3: weak film

When the film is at fault, the rust picks its spots. It starts at edges, top faces, threads, inside holes and where hands or packaging touched, and within one lot it varies with how the film was applied and which way the parts stood. Using a product meant for short indoor storage for long storage, or storing past the product's recommended protection period, belongs here as well. Take housings that were dipped, stood upright to dry and stored for a few months: when they come out, rust has bloomed only on the upper edges and inside the threaded holes, while the broad lower faces are clean.

A film does two jobs: barrier and adsorption. It blocks the path of water and oxygen, and the inhibitors in it cling to the metal surface, which is adsorption, covering the sites where the reaction would start (Revie & Uhlig, 2008). A thin film is a short barrier, so water and oxygen reach the metal sooner, and there is less inhibitor to cover the surface. That is why the same product lasts a different time depending on how thickly it went on (DoD, 1993; Revie & Uhlig, 2008).

On top of that, films do not stay even. After dipping or spraying, film drains off top areas and sharp edges and thins there, and threads and the insides of holes may not be covered at all. Handling and rubbing against packaging wear it away. Solvent-type films come in defined kinds, such as hard, soft and water-displacing films (DoD, 1993), so a film meant for short indoor storage runs out first when used for long storage or where condensation occurs.

Measuring the actual film comes first. Confirm how much film is really there by weighing before and after application or by film thickness, and check the records to see whether the storage time is within the product's recommended protection period. When products need comparing, rank them with a humidity cabinet test (ASTM International, 2024). That test is a relative comparison for cases where humidity is the main factor, and salt spray results alone do not predict real storage life well either (ASTM International, 2024, 2025).

When rust gathers on edges and top faces, revisit the coating process. Check the dilution ratio, the dip time, and which way and how long parts stand after coating, and treat threads and holes separately. If storage outlasts the film's recommended period, move to a heavier film or another type, and set an interval for checking the film during storage.

Hypothesis 4: residue under the film

Suspect what lies under the film when rust appears even in months of moderate humidity, and only on parts from a particular process or handler. The rust follows fingerprint shapes, water marks and places where liquid pooled. Think of a line where parts leave an aqueous washer still holding water and go straight into the preventive dip tank. A few weeks later each part has a ring of rust where water had pooled, and a part beside it carries a sharp, thumb-shaped rust print.

Salt drags the humidity threshold down. Salts such as sodium chloride absorb water vapour from the air until they dissolve, a property called deliquescence. Sodium chloride dissolves into droplets at about 75% relative humidity at room temperature, and even below that, water adsorbed around salt crystals can drive corrosion (Schindelholz & Kelly, 2012). So salty spots get wet at much lower humidity than clean surfaces, and the critical humidity drops (Leygraf et al., 2016; Vernon, 1935). Chloride ions from salt also break the thin protective oxide film on iron, so rust digs in as deep pits (Revie & Uhlig, 2008).

The routes in for salt are close at hand. Sweat in fingerprints carries salts, and forensic research has shown that salt in sweat drives corrosion on metals such as copper, brass and steel, leaving the print pattern behind (Bond, 2008). When water-mix coolant or aqueous cleaner is not fully rinsed or dried before the preventive goes on, that water and the salts dissolved in it are trapped under the film. The film keeps outside water out but cannot let trapped water escape, so rust proceeds beneath it (Leygraf et al., 2016; Revie & Uhlig, 2008).

The parts to examine are those just about to be preserved. Inspect them by eye and wipe them with a clean cloth to check for water and residue, and record the drying time after washing and the state of the rinse water. Check glove use at each step too. Tracing which washer and which handler the rusted parts passed through narrows the field quickly.

The remedy depends on the shape of the rust. For fingerprint shapes, stop bare-hand contact after machining and clean off existing prints before preserving. For water marks, confirm the parts are fully dry after washing before preserving, and use a water-displacing film type where water is likely to remain (DoD, 1993).

Hypothesis 5: damp, acidic packaging

Look inside the packaging when droplets sit on its inner face or the packing material feels damp on opening, or when rust follows where wooden skids, cardboard or paper touched and the same parts are fine in other packaging. Typical cases are packs sealed on a humid day, packs made with undried wood and VCI packs stored open. Parts put into an undried wooden crate on a rainy day, sealed in plastic and left in a corner of the store, would show droplets on the inside of the plastic a few weeks later, with rust running along where the wooden skids touched.

A sealed pack shuts moisture in as surely as it shuts moisture out. Packing on a humid day seals in that air along with the water held in the parts and packing materials, and when it gets colder outside, the air in the pack cools below its dew point and condensation forms on the parts (ISO, 2017; Leygraf et al., 2016). Paper, cardboard and wood take up water and release it again, so they can keep the humidity inside a pack high (Leygraf et al., 2016).

Wood brings rust by another route as well. Undried wood gives off acetic acid, the acid that makes vinegar sour, as vapour, and even at very low concentrations this vapour accelerated corrosion of many metals, steel included, above 70% relative humidity (Clarke & Longhurst, 1961). A VCI protects by spreading as vapour through a closed space and clinging to the metal, so it falls short of the concentration it needs when the pack is open, the space is too large or the material is past its use-by date. VCI compounds also suit some metals and not others (Gangopadhyay & Mahanwar, 2018).

Measure the air inside the pack directly. Put a small humidity logger or humidity indicator card inside to follow humidity during storage, and record how dry the wood is, the use-by date and seal of the VCI material, and the size of the pack space. Splitting the same parts into packaging that keeps wood away from them separates out the part the wood plays.

Changing the inside of the pack starts with the conditions at the moment of packing. Pack on dry days with dry parts and dry materials, and add a desiccant to sealed packs. Where rust appears at points of contact with wood, use dried wood or put a barrier between part and wood (Clarke & Longhurst, 1961). With VCI, check sealing, space size and target metal against the supplier's guidance (Gangopadhyay & Mahanwar, 2018).

Testing the hypotheses

A rusted part is a record in itself. Rather than investigating all five hypotheses at once, photograph the rust's position and shape where the part is found, and first sort it: even and light, concentrated on top faces and edges, shaped like fingerprints or water marks, or where packaging touched. That sorting alone cuts the suspects to two or three.

If there is packaging, check it as it opens. Droplets, dampness or contact with wood or cardboard put hypothesis 5, the air inside the pack, and hypothesis 2, condensation, first in line (Clarke & Longhurst, 1961; ISO, 2017). Rust shaped like fingerprints or water marks points to hypothesis 4; trace back through handling and the washing and drying steps (Bond, 2008). Rust gathered on edges, threads and top faces points to hypothesis 3; check the coating method, the film amount and the storage time (DoD, 1993).

If even, light rust is what remains, settle it with records of the store's air. Logging humidity, dew point and part temperature together for a few weeks separates long stretches of high humidity from parts dropping below the dew point: the first means hypothesis 1, the second hypothesis 2 (ISO, 2017; Vernon, 1935).

Once one cause is fixed, the last check is a comparison. Split parts from one lot between the corrected conditions and the old ones, store them side by side, and compare the rust after the same period. If only the changed side stays clean, the cause was most likely the right one. Read any humidity or salt spray test used to choose a new product as a relative comparison only (ASTM International, 2024, 2025).

The hypotheses often overlap. A thin film holds for most of the year and fails in the condensation season, and salt under the film shows itself when humidity rises. In such cases pair the sources of water, hypotheses 1, 2 and 5, with the weak points in the film, hypotheses 3 and 4, and start with the change that is easiest to make and likely to matter most.

Limits and cautions

Aluminium, copper alloys and galvanised parts form different corrosion products from steel and suit different inhibitors (Clarke & Longhurst, 1961; Gangopadhyay & Mahanwar, 2018), and special settings such as the surroundings of chemical plants are not covered by the international standard's general classification (ISO, 2012). If rust has pitted deeply or sits on a functional surface, quality staff decide whether the part can be reused.

Use accelerated tests for relative comparison, and do not convert their results directly into storage life (ASTM International, 2024, 2025). Solvent-type preventives carry flammable vapour and inhalation risks, so follow the product's safety data sheet, the SDS, and provide ventilation and protective equipment. When packaging changes substantially, or long transport such as export is involved, it is safer to set the conditions together with the preventive supplier's technical staff.

Sources

  1. ASTM International. (2024). ASTM D1748-24, Standard test method for rust protection by metal preservatives in the humidity cabinet. https://store.astm.org/d1748-24.html
  2. ASTM International. (2025). ASTM B117-25, Standard practice for operating salt spray (fog) apparatus. https://store.astm.org/b0117-25.html
  3. Bond, J. W. (2008). Visualization of latent fingerprint corrosion of metallic surfaces. Journal of Forensic Sciences, 53(4), 812–822. https://doi.org/10.1111/j.1556-4029.2008.00738.x
  4. Clarke, S. G., & Longhurst, E. E. (1961). The corrosion of metals by acid vapours from wood. Journal of Applied Chemistry, 11(11), 435–443.
  5. Evans, U. R. (1965). Electrochemical mechanism of atmospheric rusting. Nature, 206, 980–982. https://doi.org/10.1038/206980a0
  6. Gangopadhyay, S., & Mahanwar, P. A. (2018). Recent developments in the volatile corrosion inhibitor (VCI) coatings for metal: A review. Journal of Coatings Technology and Research, 15(4), 789–807. https://doi.org/10.1007/s11998-017-0015-6
  7. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  8. International Organization for Standardization [ISO]. (2017). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application. https://www.iso.org/standard/58061.html
  9. Leygraf, C., Odnevall Wallinder, I., Tidblad, J., & Graedel, T. (2016). Atmospheric corrosion (2nd ed.). Wiley. ECS Series of Texts and Monographs. ISBN 978-1-118-76227-1
  10. Revie, R. W., & Uhlig, H. H. (2008). Corrosion and corrosion control: An introduction to corrosion science and engineering (4th ed.). Wiley. https://doi.org/10.1002/9780470277270
  11. Schindelholz, E., & Kelly, R. G. (2012). Wetting phenomena and time of wetness in atmospheric corrosion: A review. Corrosion Reviews, 30, 135–170.
  12. Stratmann, M., & Streckel, H. (1990a). On the atmospheric corrosion of metals which are covered with thin electrolyte layers—I. Verification of the experimental technique. Corrosion Science, 30(6–7), 681–696.
  13. Stratmann, M., & Streckel, H. (1990b). On the atmospheric corrosion of metals which are covered with thin electrolyte layers—II. Experimental results. Corrosion Science, 30(6–7), 697–714.
  14. U.S. Department of Defense [DoD]. (1993). MIL-PRF-16173E, Corrosion preventive compound, solvent cutback, cold-application. Interim Amendment 2, 2017. https://everyspec.com/MIL-PRF/MIL-PRF-010000-29999/MIL-PRF-16173E_5815/
  15. Vernon, W. H. J. (1935). A laboratory study of the atmospheric corrosion of metals. Part II.–Iron: The primary oxide film. Part III.–The secondary product or rust. Transactions of the Faraday Society, 31, 1668–1700. https://doi.org/10.1039/TF9353101668

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.