Bubbles or cracks in sealant are usually blamed on the product and met with a different sealant, but if the joint and site conditions stay the same, the new product can show the same defect. What actually causes them can be gas trapped during cure, gas from the backer rod, a bead that is too deep, joint movement during cure, faulty joint design or weathering of the sealant, and two or more can overlap.

Sometimes, a few days after a joint is filled, the sealant bead is blistered in places or peppered with small holes. A joint that looked sound after application can split along its centre months or years later, or pull away from the wall and open a gap. Then it may be only when water stains appear on an inside wall that anyone looks at the joint again.

Bubbles thin the sealant's cross-section so that strain concentrates there, and a bubble that bursts at the surface opens a path for water. Cracks lead straight to leaks and rework. Rework means cutting out the old sealant and preparing the surfaces again, so it takes more time and money than the first application. Unless the cause is found, the same defect can return in the reworked joint.

Sealant fills the joint between two parts to keep out water and air, and stretches and compresses as the parts move with temperature and load. Standards rate sealants by how much movement they can take. Classes are set by the share of joint width the sealant can stretch and compress, such as 25% or 20% (ISO, 2002), and another standard sets movement classes and test methods for elastomeric sealants (ASTM International, 2024). These ratings assume fully cured sealant in a correctly shaped joint. One-part sealants, however, usually cure from the outside in with moisture from the air (Petrie, 2007), so the days before full cure and the shape of the joint weigh heavily on the result.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The first step never changes: cut out a section at the defect, find the day's temperature, humidity, rain and substrate condition in the application record, and set them beside the application conditions in the sealant's technical data sheet, the TDS.

Hypothesis 1: trapped carbon dioxide

Start with this hypothesis if polyurethane sealant went in on a hot, humid day, or onto a wet surface just after rain. Typical places are substrates that hold water, such as concrete, façade work in the rainy season and floor joints warmed by direct sun. One example is a concrete joint soaked by morning rain that looked dry by the afternoon and was filled with polyurethane sealant there and then. The next day the bead is swollen in places, and pressing it shows hollows that collapse under a finger.

What fills the swelling is carbon dioxide from the cure reaction. One-part polyurethane sealant is a polymer whose chain ends carry isocyanate groups, which react readily with water and amines. When moisture from the air enters, an isocyanate group reacts with water to give an amine and carbon dioxide, and that amine reacts with another isocyanate group to join chains through urea links; that is the cure. In urethane foam the same reaction gives off enough gas to serve as the blowing agent (Akindoyo et al., 2016; Petrie, 2007).

Normally moisture enters slowly, so carbon dioxide forms slowly too and most of it escapes at the surface. When a wet substrate puts water straight against the bottom of the bead, or heat and humidity speed the reaction, gas forms all at once. In experiments on a moisture-cure silicone, too, temperature and humidity acted together to speed cure (Elsmore & De Focatiis, 2021). If a cured skin has already formed on top, the gas cannot get out and is trapped as bubbles. The same reason explains why uncured polyurethane that meets water can bubble or swell (Akindoyo et al., 2016; Petrie, 2007).

Look first at the shape of the bubbles in the section. Small bubbles spread evenly through the bead, especially near the substrate, with the bead swollen and lumpy, make this hypothesis the strong one. Find the day's air temperature and relative humidity in the records, and whether it rained within hours of application; for concrete joints, also check whether the surface was wet at the time and whether sun-warmed slab was sending vapour up. Silicone and silyl-modified sealants, known as MS or STP, give off small molecules such as alcohol rather than carbon dioxide as they cure, so they show fewer such bubbles in the same conditions (Petrie, 2007). If a different type shows the same bubbles, move on to the next hypothesis.

The remedy lies in keeping water and heat away. Apply to dry substrates, and postpone when rain is forecast or the substrate is hot from direct sun. In humid seasons or on sites that stay damp, review with the supplier whether a silicone or silyl-modified type, which releases no carbon dioxide, suits better. Mix two-part polyurethane by the stated method and time so that no air is folded in. A bubbled bead is safer cut out and reapplied over the affected length than patched in spots.

Hypothesis 2: backer rod outgassing

Large, scattered bubbles point to the backer rod at the bottom of the joint. They tend to occur where backing is pushed in by hand in a hurry, where crews press it in with sharp tools, and on façades in strong sun where joints warm up easily. On a façade joint where the backing was pressed in with a screwdriver tip before sealing, the afternoon sun the next day can raise round lumps at regular intervals along the bead.

Backer rod is a round foam placed in the joint to set the sealant depth and keep the bottom of the bead from bonding, and cold-applied sealants often use closed-cell polyethylene foam, whose cells are sealed off from each other. The backing standard classifies it as closed-cell, open-cell or a mix of the two, and sets outgassing properties for each type (ASTM International, 2023). Closed cells hold gas, so if the rod is punctured by a sharp tool or squeezed hard enough to burst cells during installation, that gas escapes.

Gas released while the sealant is still soft rises, pushes the sealant up and leaves voids. When sun warms the joint, gas in the cells expands and makes this worse. There is even a dedicated test method that measures, under heat and compression, how many voids a punctured backing creates in uncured sealant. It aims to catch defective backing, damage in shipping and rough installation, and states that voids from air trapped during application or from incompatible materials must be told apart (ASTM International, 2019).

Pulling out the backing at the defect is the surest check. If the section shows large bubbles rising from right above the backing, and the removed rod has tears or flattened sections, this is the hypothesis. Ask too whether the surface lumps appeared after the joint warmed up, and what tool the installer used to push the rod in. If the backing is intact but voids sit irregularly through the bead, look at air trapped during application: pulling the gun instead of pushing it, or skipping tooling, leaves air between the sealant and the joint walls.

From the next job on, change how the backing is handled. Choose a rod slightly larger in diameter than the joint width, push it in with a blunt roller, never use sharp tools such as a screwdriver or blade tip, and do not stretch or twist it in. Push the gun forward while applying, and tool the bead before it skins to press out air. For joints in strong sun or where backing is easily damaged, review with the supplier whether open-cell or mixed-cell backing fits better; open-cell foam can hold water, though, so for joints exposed to water check the guide on joint sealant use together with the supplier's advice (ASTM International, 2025).

Hypothesis 3: excess bead depth

This hypothesis comes up for joints where the backing is missing or set too deep and the sealant fills a thick section, for deep gaps filled with sealant alone, and for work in cold, dry seasons. A deep gap filled with sealant in one go in winter may, a few days later, feel firm outside while a cut brings out sticky paste from inside. Bubbles or fine splits may show on the surface as well.

The inside and outside differ like this because of the direction in which moisture-cure sealant sets. One-part moisture-cure sealant cures first at the surface that meets the air, and once a cured layer forms, moisture has to diffuse through it to reach the inside, so cure slows with depth (Petrie, 2007). Cure rate depends on temperature and on the moisture in the air, and slows sharply when it is cold and dry (Elsmore & De Focatiis, 2021), so a thick section takes a long time to cure through even after the surface has set.

In a deep bead this gap leads to two defects. With polyurethane, carbon dioxide formed late inside is blocked by the cured top layer and stays as bubbles (Akindoyo et al., 2016). And if the joint moves while only the top has cured and the inside is soft, strain concentrates in the stiff top layer and the surface splits. A thick bead also passes more force to the substrate for the same change in width, so the bond line lets go more easily. That is why joint guides set a width-to-depth ratio and minimum and maximum depths (ASTM International, 2022; ASTM International, 2025).

A ruler is all it takes. Cut a section, measure the sealant depth and compare it with the depth recommended in the TDS. If the inside is still tacky or dents under a fingernail after several days, cure is incomplete, and missing or deeply set backing explains why the depth grew. Check the temperature and humidity around the time of application as well, because in winter the same depth cures much more slowly (Elsmore & De Focatiis, 2021).

Set the depth with backing, not with sealant. Make the joint shallow with backing to keep to the width-to-depth ratio the supplier recommends, and do not fill a deep gap thickly in one pass. Where a deep gap that is not a joint must be filled, consider a two-part product made to cure evenly through a deep section. In cold, dry seasons allow plenty of cure time, and keep load and water off the bead until it has fully cured.

Hypothesis 4: movement during cure

This hypothesis fits joints whose surface wrinkles or splits along the centre within days of application while the inside is still soft. It tends to occur in joints between parts that move a lot with temperature, such as faces in strong sun, dark panels and metal curtain walls. Take a joint between dark metal panels filled at midday in high summer: at night the panels cool and the joint opens, and by the third morning a long wrinkle may run down the middle of the bead.

Partly cured sealant is not yet an elastomer. Façade joints open and close with day and night temperature from the moment the sealant goes in, while the sealant slowly turns from a flowing paste into an elastomer (Petrie, 2007). A shape stretched while soft cures in place, leaving the bead thin or wrinkled, and a large stretch while only the top has cured tears the surface (Matsumoto, 1992; White et al., 2010).

Experiments and real buildings tell the same story. In outdoor exposure tests, failures caused by joint movement during cure fell into four patterns, and these matched failures observed on buildings in service (Matsumoto, 1992). In laboratory work on a one-part silicone sealant, the key factor for performance was how far cure had progressed when movement began (White et al., 2010). The same sealant, in other words, ends up differently depending on when movement starts.

The time of application and the day's temperatures are the clue. Find in the records when the sealant went in and what that day's high and low were, and see whether defects cluster on sunlit faces or dark panels. Measuring joint width in the morning and the afternoon shows the daily movement directly and makes the call easier. A section still soft inside, with only the surface wrinkled or torn, adds weight to this hypothesis.

The first remedy is to move the time of application. Fill high-movement joints when the joint is near its mean width, usually when the temperature is moderate. Applied at the midday peak, the joint opens wide at night and pulls on the soft sealant. A faster-curing product or a two-part sealant shortens the soft period. Cut out failed lengths once they have fully cured, and reapply at a time when the same conditions will not recur.

Hypothesis 5: faulty joint design

If the same joint cracks again after rework, look at the joint rather than the sealant. It happens in joints designed too narrow, on façades whose parts move a lot, and in joints filled to the bottom with no backing or tape. Cut open a joint that splits in the same place after every repair, and the sealant is bonded hard to the bottom with no backing, with the tear running up from a bottom corner.

The movement a sealant can take is set as a share of joint width: a 25% class sealant can stretch and compress by 25% of the joint width (ISO, 2002). If the real movement, adding thermal expansion, swelling and shrinkage with moisture, and construction tolerance, goes beyond that range, the sealant fatigues under repeated load and splits or pulls away from the substrate. A standard guide gives equations for calculating the joint width and depth needed from this movement and the tolerances (ASTM International, 2022).

The joint's shape matters too. When sealant is bonded only to the two sides, the whole bead stretches evenly like a rubber band. With three-sided adhesion, where it is bonded to the bottom as well, the bottom cannot stretch, strain concentrates at a corner, and a tear starting there spreads upward. That is why the guide on joint sealant use directs that the bottom bond be broken with backing or bond-breaker tape (ASTM International, 2025).

Where the crack started is the fork in the road. Adhesive failure, with the bead parting along the substrate edge, points to surface preparation, primer or excessive movement; cohesive failure starting mid-bead or at a bottom corner points to movement beyond capacity or three-sided adhesion. Check in the section whether backing or tape is present and whether the sealant is bonded to the bottom, then measure joint width at several points and compare it with the design width and with the movement class in the TDS.

Calculate before reworking. Work out the real movement by the method in the standard guide and confirm that the joint is wide enough (ASTM International, 2022); if it is too narrow, use a low-modulus sealant, one that stretches under little force, with a higher movement class, or widen the joint. Break the bottom bond with backing or bond-breaker in every movement joint. Clean dust and oil from the substrate, and apply the primer the supplier specifies within the stated window.

Hypothesis 6: weathering

Weathering is the suspect when fine cracks spread across a joint some years after application. It shows first on façades that take long hours of sun, such as south and west elevations, and in roof and parapet joints that see rain and sun by turns. An inspection of a south façade may find the sealant covered in a shallow network of cracks like a turtle's shell, harder than when new and leaving white powder on a fingertip, while the north joints of the same building are relatively sound.

Sealant in an outdoor joint faces ultraviolet light, heat, water and repeated movement all at once. Ultraviolet light and heat break polymer chains or add crosslinks, making the surface layer harder and less stretchy, and water weakens the interface between sealant and substrate (Petrie, 2007). A technical committee of RILEM, the international association for construction materials research, named cyclic movement, sunlight, temperature change and water as the main factors in sealed joint failure (RILEM TC 139-DBS, 2001), and work that applied the four factors singly and together showed that the effect of each, and the synergy between them, can be put into numbers (White et al., 2012).

The hardened top layer cannot stretch as far as the softer material beneath, so every time the joint opens, fine cracks form at the surface and slowly deepen. An international standard exposes sealant to heat, water and artificial light through glass, then extends it to judge adhesion and cohesion, and it is used to compare this weathering resistance between products (ISO, 2025).

Compare sunlit and shaded faces side by side. If joints of the same product and the same age have crazed, hardened, faded or chalky surfaces only on the sunny side, this hypothesis is the strong one. Cut a section and see whether the cracks stay in the surface layer or run through the full depth, and whether the bead has pulled away from the substrate anywhere.

If the cracks stay at the surface and the bond is sound, there is no need to rush. The immediate leak risk is low, so set an inspection interval and watch how it develops. Where cracks run through the full depth or the bead has come away from the substrate, cut it out and reapply. Choose the rework product by asking the supplier for weathering test results that match the outdoor exposure, and use a type with proven weather resistance in joints under strong ultraviolet light.

Testing the hypotheses

There is no need to look at all six hypotheses at once. The first thing to settle is when the defect appeared. Within days or weeks of application, look first at hypotheses 1 to 4, which concern what happens during cure; after years, look first at hypotheses 5 and 6, joint design and weathering. Pulling the day's temperature, humidity, rain, substrate condition and tools from the application record makes every later judgement easier.

Next comes the section. Small bubbles spread evenly through the bead point to hypothesis 1; large bubbles starting right above the backing point to hypothesis 2. If the backing is intact and the voids are scattered irregularly, consider air trapped during application separately (ASTM International, 2019). A bead deeper than recommended and still soft inside is hypothesis 3 (Petrie, 2007); a soft inside with only the surface wrinkled or torn is hypothesis 4 (White et al., 2010).

For cracks, look at where they start. A start at a bottom corner with the bottom bonded, or a joint narrow for the calculated movement, is hypothesis 5 (ASTM International, 2022; ASTM International, 2025). Where possible, measure joint width morning and afternoon and compare the daily movement with the design width and the product's movement class. Then compare sunlit and shaded faces; surface crazing and hardening on the sunny side alone separate out the share of weathering, hypothesis 6 (White et al., 2012).

After the fix, return to the same joint. Only when the reworked length has been checked a few days after application, and again after its first summer and first winter, without the same defect returning, can the cause be called found.

The hypotheses often overlap. A polyurethane bead applied too deep just before summer rain brings hypotheses 1 and 3 into play together. In such cases it is efficient to fix first what rework can change, namely joint depth, backing and timing, and only then review whether to change the sealant type.

Limits and cautions

Movement classes, width-to-depth ratios and the temperature and humidity range for application differ by product, so take the figures from that product's TDS. Structural silicone glazing, fire-rated joints, areas in contact with food or medical use, and joints exposed to fuel or chemicals need their own standards and design review. If a joint is far narrower than the calculation requires, or the parts themselves are cracking, the problem may lie in the structure rather than the sealant, so consult the designer. If the cause is hard to pin down or a large area needs rework, ask the sealant supplier for technical support and a site inspection.

Polyurethane sealants and primers may contain isocyanates, which can sensitise the skin and airways and cause occupational asthma (NIOSH, 1996; OSHA, n.d.). Before application or removal, read the safety data sheet, the SDS, and provide ventilation, gloves, eye protection and, where needed, respiratory protection. Do not burn old sealant off or melt it out with a hot wire.

Sources

  1. Akindoyo, J. O., Beg, M. D. H., Ghazali, S., Islam, M. R., Jeyaratnam, N., & Yuvaraj, A. R. (2016). Polyurethane types, synthesis and applications: A review. RSC Advances, 6, 114453–114482. https://doi.org/10.1039/C6RA14525F
  2. ASTM International. (2019). ASTM C1253-14(2019), Standard test method for determining the outgassing potential of sealant backing. https://store.astm.org/c1253-14r19.html
  3. ASTM International. (2022). ASTM C1472-16(2022), Standard guide for calculating movement and other effects when establishing sealant joint width. https://store.astm.org/c1472-16r22.html
  4. ASTM International. (2023). ASTM C1330-23, Standard specification for cylindrical sealant backing for use with cold liquid-applied sealants. https://store.astm.org/c1330-23.html
  5. ASTM International. (2024). ASTM C920-18(2024), Standard specification for elastomeric joint sealants. https://store.astm.org/standards/c920
  6. ASTM International. (2025). ASTM C1193-25, Standard guide for use of joint sealants. https://store.astm.org/c1193-25.html
  7. Elsmore, M. T., & De Focatiis, D. S. A. (2021). Combined roles of temperature and humidity on cure of a silicone elastomer. Polymer Testing, 93, 106967. https://doi.org/10.1016/j.polymertesting.2020.106967
  8. International Organization for Standardization [ISO]. (2002). ISO 11600:2002, Building construction: Jointing products: Classification and requirements for sealants. Including Amd 1:2011. https://www.iso.org/standard/26328.html
  9. International Organization for Standardization [ISO]. (2025). ISO 11431:2025, Building and civil engineering sealants: Determination of adhesion and cohesion properties of sealants after exposure to heat, water and artificial light through glass. https://www.iso.org/standard/88024.html
  10. Matsumoto, Y. (1992). The effect of building joint movements on outdoor performance of sealants during their cure. ASTM International symposium paper, STP. https://store.astm.org/stp24233s.html
  11. National Institute for Occupational Safety and Health [NIOSH]. (1996). Preventing asthma and death from diisocyanate exposure (DHHS [NIOSH] Publication No. 96-111). https://www.cdc.gov/niosh/docs/96-111/
  12. Occupational Safety and Health Administration [OSHA]. (n.d.). Isocyanates: Health hazards and solutions. U.S. Department of Labor. https://www.osha.gov/isocyanates
  13. Petrie, E. M. (2007). Handbook of adhesives and sealants (2nd ed.). McGraw-Hill. ISBN 9780071479165
  14. RILEM TC 139-DBS. (2001). Durability test method: Determination of changes in adhesion, cohesion and appearance of elastic weatherproofing sealants for high movement façade joints after exposure to artificial weathering. Materials and Structures. https://www.rilem.net/images/publis/1282.pdf
  15. White, C. C., Hunston, D. L., & Williams, S. (2010). Studies on the effect of movement during the cure on the mechanical properties of building joint sealant. Polymer Engineering and Science. https://www.nist.gov/node/601556
  16. White, C. C., Hunston, D. L., Tan, K. T., & Filliben, J. J. (2012). A systematic approach to the study of accelerated weathering in building joint sealants. Journal of ASTM International, 9(5). https://www.nist.gov/node/586656

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.