KALTECKOREA

BlogApplication notes

Why are there bubbles and voids in the bond line?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Adhesives

Applying a thicker layer or pressing harder is the usual response to bubbles in a bond line, but a void is gas that entered or formed before the adhesive set and could not get out, so unless the source of that gas is known, changing the amount or the pressure leaves it to recur. What actually lies behind it can be air taken in during mixing and dispensing, carbon dioxide from urethane reacting with moisture, gas released by the substrate, the bead pattern and closing order, or skipped degassing and the wrong storage temperature, and sometimes two or more at once.

Background

Cut open a test part and the bond line section is riddled with holes of all sizes. On a transparent part, silvery froth shows through from the moment it is bonded, and ultrasonic inspection flags empty areas across the bond line. Voids shrink the area that carries load; where the bond also seals, connected voids become a leak path; and in resin covering electronics, bubbles that bridge conductors can lower insulation (NASA, 2016). Parts are also returned for appearance or rebuilt after failing inspection.

How harmful a void is depends on its size, its location and the structure. Analysis has shown that thin structures tolerate quite large flaws, while thick joints are sensitive to both large voids and fine porosity (Hart-Smith, 1982). So bubbles are neither automatically a reject nor something to ignore; judge them against the acceptance criteria for that part.

A void is, in the end, gas that was inside the adhesive before it set. The gas either comes in from outside during mixing and application, or forms inside the adhesive or the substrate. The speed at which a bubble rises through a liquid grows with the square of its size and falls with viscosity (Bird et al., 2002), so a bubble that would escape from a thin liquid barely moves in a viscous adhesive and is set in place.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: section a sample with voids and record bubble size, shape and position, then log the mixing and dispensing method, material storage temperature, workshop humidity and cure conditions, and compare them with the adhesive's technical data sheet, the TDS.

Hypothesis 1: air mixed or pumped in

Air gets in when two parts are hand-mixed with a spatula in a cup, when a power stirrer runs fast, when the first bead is not discarded after a cartridge change, when a drum runs low and the pump draws air, or when a joint on the suction side of a meter-mix machine is loose. At the bench, a two-part epoxy is sometimes poured into a cup and stirred in a hurry. The clear mixture quickly turns cloudy, and in that state it goes straight onto the part.

Each time a stirring blade breaks the surface it folds air in and chops it up, and the mixture turns cloudy because those fine bubbles scatter light. The smaller the bubble, the more its rise speed falls, with the square of its size, so in a viscous adhesive they barely escape within the pot life. That is why the workmanship standard for polymer application on electronic assemblies requires stirring and mixing to be done carefully to minimise entrapped air, and allows high-viscosity materials to be deaerated (NASA, 2016). On the dispensing side, air left at a cartridge outlet or behind a piston, or drawn in by a pump, comes out in pockets within the bead.

The shape of the bubbles in the section is the first clue. Small, even, round bubbles spread throughout the bond line send the first look to mixing; large bubbles appearing here and there along the bead, or clustered in parts made just after a cartridge change, send it to dispensing. Dispensing a bead onto clear film or a glass plate and holding it to the light shows the state straight after mixing. On a meter-mix machine, check the suction hoses and joints and how much is left in the drum as well.

If the air came in during mixing, cut back on hand mixing first. Move to cartridges with static mixing nozzles or a meter-mix machine; where hand mixing is unavoidable, mix slowly by scraping the bottom and sides so the blade never breaks the surface, then degas by a method the TDS allows. Before fitting the mixing nozzle, extrude a little until both sides flow evenly to purge the air, and discard the first bead after the nozzle is fitted. Set a low-level alarm so the pump is switched before the drum runs dry.

Hypothesis 2: CO2 from urethane

These bubbles arise in one-part urethanes that cure with moisture from the air, and in two-part urethanes whose polyol side has taken up moisture. They stand out in the rainy season or a humid workshop, with drums used with the lid open, with fillers that hold moisture, and in thick layers. Consider a week of steady rain in which a polyol drum whose lid was not properly closed went into use. The bond line has turned into a sponge full of fine froth, with far more foam where it built up thick than where it was spread thin.

A urethane's isocyanate groups, on meeting water, pass through unstable carbamic acid and split into an amine and carbon dioxide, and the amine then reacts with more isocyanate to form urea. In foam making, this carbon dioxide is the blowing gas used on purpose (Szycher, 2012). Structural urethane adhesives come as one-part moisture-cure and two-part mixed systems (Burchardt, 2010); in one-part systems the reaction with moisture is the cure itself, so they always make this gas, while two-part systems make it when water that should not be there has come in with the polyol or filler. There is a standard test method just for the water content of polyols precisely because isocyanates react with water (ASTM International, 2018). The thicker the layer, the longer the path for gas to reach the surface, so the bubbles formed are easily trapped.

These bubbles are usually fine, even and clustered like foam, and grow with thickness and on humid days. So the first check is to match the workshop humidity log for days with many bubbles against the dates drums were opened. Measure the water in the polyol and fillers by Karl Fischer titration and compare it with the supplier's specification, and compare bubbles in bonds made on dry and humid days, thin and thick.

Once moisture is the likely cause, start by keeping the material away from water. Open drums and tins only when in use, guard against moisture with a desiccant breather or a nitrogen blanket, and dry fillers to the supplier's conditions. For one-part systems keep to the maximum thickness and humidity range in the TDS, and where a gap must be filled thicker than that, review a two-part system or another cure mechanism with the supplier.

Hypothesis 3: gas from the substrate

Here it is the substrate that gives off gas. It happens when materials that hold water or air inside, such as moist composites, wood, concrete, porous castings and foams, are bonded with heat cure, or when adhesive covers a cleaning solvent before it has fully flashed off. Suppose a carbon fibre composite part that sat for weeks in a humid store is bonded with a heat-curing adhesive. Sectioned after the oven, the part shows bubbles not in the middle of the bond line but lined up as hemispheres along the interface on the composite side.

Composite resin slowly absorbs moisture from the air, and when heat is applied to cure the adhesive, that moisture moves into the adhesive. A study of bonded repairs to carbon fibre composites explains that this moisture can cause excessive voiding, plasticisation, cure interference and a weak interface, and reports that at the same moisture content, joints dried before bonding performed better than undried ones (Bond et al., 1998). An earlier study also found that laminates holding more moisture gave lower joint strengths, to a degree that depended on the adhesive (Parker, 1983). Air in the pores of wood or castings expands when heated and is pushed into the adhesive, and solvent that has not dried vaporises with the cure heat. Because the gas comes out of the interface, the bubbles stay attached to that face.

The clue is where the bubbles sit. If they cling as hemispheres to the interface of one substrate and are scarce on the other face and in the middle of the bond line, this hypothesis is the strong candidate. Split substrates from one lot into dried and undried, bond them under the same conditions and compare, and weigh coupons before and after drying to gauge the moisture. If bubbles fall when the same joint is cured at room temperature, the heat was most likely what drew the gas out.

If the substrate is the cause, empty the gas source before bonding. Dry moist composites and parts under set conditions before bonding; in polymer application on electronic assemblies, too, a bake to remove moisture before application is to be defined and recorded (NASA, 2016). Seal porous faces first with a primer or a thin first coat, and let cleaning solvent flash off for the time the supplier recommends before applying adhesive. For heat cure, review with the supplier a gentler heating rate and staging within what the TDS allows.

Hypothesis 4: bead and closing order

Look at this hypothesis on panels bonded over a wide area, parts with a closed loop of bead around the edge, processes that cover dots or several bead lines at once, beads laid as flat ribbons, and work where two plates are lowered flat onto each other in one go. Imagine a rectangular panel with a bead run once around its perimeter and a few more lines across the middle, then the top plate lowered level and pressed. Pull it apart and each space between bead lines holds one flat, irregular void.

A pressed bead spreads sideways and has to push the air between beads out to the edge. If beads meet first and form a loop, the air inside loses its way out and is trapped, and a bead closed around the perimeter blocks the exit from the start. Flat ribbon beads, or a plate lowered flat in one go, cover a wide area the moment the adhesive touches and trap air easily. The workmanship standard for electronic assemblies likewise explains that bubbles usually come from air trapped beneath components (NASA, 2016). The effect of voids trapped this way depends on where they are. In an analysis of lap joints, a void in the middle of the overlap barely changed the peak stresses even when fairly large, because stress in the joint concentrates at the two ends of the overlap (Chadegani & Batra, 2011).

These voids can be recognised by their shape. They are flat with ragged edges rather than round, and sit regularly between the paths along which beads were laid. Pressing a glass plate onto the same bead pattern shows by eye where air is trapped, and repeating the test while changing the closing order and bead shape picks the better method. On production parts, ultrasonic inspection finds voids and disbonds in the bond line without destroying the part (Adams & Drinkwater, 1997).

Redraw the bead so the air has a way out. Replace a closed perimeter loop with lines open at the ends, use one thick central line or a wave pattern open towards the edges instead of many lines, and lay a bead with a peaked triangular or round section rather than a flat ribbon. When closing, let one end touch first and lower the other side like a hinge so the adhesive spreads in one direction. For lap joints, fill the ends well so that no voids fall there.

Hypothesis 5: degassing and storage

Suspect this hypothesis when the degassing step was skipped for a high-viscosity or heavily filled material, when material kept in a cold store is used straight away without warming, or when settled filler was stirred back in hard and the material used at once. In winter, a cartridge taken from an unheated store and put straight into the gun dispenses a stiff bead that takes effort to push, and the morning's parts have unusually many bubbles. In the afternoon, with cartridges warmed by the workshop air, the bubbles fall noticeably.

Cold material is more viscous, so the same bubble rises more slowly, and dispensing and mixing take more force, which also makes it easier to fold air in. Degassing a high-viscosity material is the step that deliberately removes these bubbles. Under vacuum, bubbles swell, so their rise speed increases with the square of their size and they reach the surface and burst (Bird et al., 2002). Degassing has a cost, though. The workmanship standard for electronic assemblies says high-viscosity materials may be deaerated to remove entrapped air but may lose volatile ingredients in the process, requires encapsulants to be vacuum degassed before application, and notes that even single-part materials may need stirring when filler settles (NASA, 2016). Stirring and degassing go together, so if degassing is skipped after stirring, the air stirred in stays.

Match the storage temperature of the material and the time it spent in the workshop before use against the records, and see whether days with many bubbles cluster on cold days or in the hours just after material was brought out. Splitting the same material into degassed and not, and conditioned to workshop temperature and cold, then comparing them in a clear cup or on a glass plate shows the difference at once. If there is degassing equipment, check that its vacuum level and time match the TDS conditions.

If storage and degassing are the cause, tie the two together in the procedure. Keep the material at the TDS storage temperature and condition it to workshop temperature for a set time before use. Remix settled material slowly by the method the supplier recommends, and after mixing degas at the vacuum level and for the time in the TDS, without overrunning the time so as not to lose volatile ingredients. Warming a two-part system can shorten its pot life, so set the warming temperature within the TDS range as well.

Finding the cause

There is no need to investigate all five hypotheses separately. One cross-section tells the most. Cut a voided sample in a few places and photograph bubble size, shape and position, and the shape alone narrows the candidates to two or three. For production parts that cannot be cut, look at the void distribution with ultrasonic inspection.

Small round bubbles spread evenly through the bond line point to air mixed in or carbon dioxide from urethane; if they cluster like foam and grow with thickness and on humid days, the urethane and moisture are the likely pair. Bubbles clinging as hemispheres to one interface point to gas from the substrate, and flat, ragged voids lying regularly between beads to the bead pattern and closing order. Bubbles that rise on cold days or just after material comes out of storage point to storage temperature and degassing.

Next come the records. Splitting mixing method, cartridge change times, the dates material was opened and its storage temperature, workshop humidity, substrate storage and cure temperature into days with many bubbles and days with few reveals the condition the bubbles move with.

If that still does not settle it, run control trials that change one thing at a time. Make reference samples with material conditioned to workshop temperature and degassed, dispensed through a static mixing nozzle, on dried substrates, with a bead pattern that lets air out, then return the conditions to line values one at a time and find where bubbles reappear. Change only one thing at a time, or there is no telling which one worked. The final check is to section a set number of production parts made under the new conditions, or inspect them ultrasonically, and see whether they fall within the part's acceptance criteria.

The hypotheses can overlap. Mixing cold urethane hard on a humid winter morning and laying it thick adds moisture, mixed-in air and high viscosity to the bubbles all at once. In such cases, put material handling right first, meaning moisture exclusion, temperature conditioning and degassing, to cut the round bubbles, then look at the flat voids or interface bubbles that remain from the bead pattern and substrate side. While material-side bubbles are numerous, the effect of a new bead pattern cannot be compared fairly.

Limits and cautions

Acceptable bubble size and quantity, maximum application thickness, degassing conditions, storage temperature and cure conditions differ by product and part, so numeric decisions follow the adhesive's TDS and the part's acceptance criteria. Voids in safety-related joints, such as in aircraft, vehicles or building structures, should not be accepted on floor judgement alone; refer them to the specified non-destructive inspection and to the design engineer.

Isocyanates in urethane adhesives can cause asthma and sensitisation when breathed in or in contact with skin, so provide ventilation, respiratory protection and gloves (OSHA, n.d.). For vacuum degassing, confirm the container can take the vacuum and leave enough headroom that the material does not overflow as it swells, and keep within oven temperature limits for heat cure and substrate drying. Handle adhesives and cleaning solvents according to the product's safety data sheet, the SDS.

Sources

  1. Adams, R. D., & Drinkwater, B. W. (1997). Nondestructive testing of adhesively-bonded joints. NDT & E International, 30(2), 93–98. https://doi.org/10.1016/S0963-8695(96)00050-3
  2. ASTM International. (2018). ASTM D4672-18, Standard test method for polyurethane raw materials: Determination of water content of polyols. https://store.astm.org/d4672-18.html
  3. Bird, R. B., Stewart, W. E., & Lightfoot, E. N. (2002). Transport phenomena (2nd ed.). Wiley.
  4. Bond, D., Swan, G., Bader, M., & Smith, P. (1998). The effect of matrix moisture content on the repair of carbon fibre reinforced epoxy. In Proceedings of the 21st Congress of the International Council of the Aeronautical Sciences (ICAS-98-4.4.3). https://www.icas.org/icas_archive/ICAS1998/ABSTRACTS/443.HTM
  5. Burchardt, B. (2010). Advances in polyurethane structural adhesives. In D. A. Dillard (Ed.), Advances in structural adhesive bonding (pp. 35–65). Woodhead Publishing. https://doi.org/10.1533/9781845698058.1.35
  6. Chadegani, A., & Batra, R. C. (2011). Analysis of adhesive-bonded single-lap joint with an interfacial crack and a void. International Journal of Adhesion and Adhesives, 31(6), 455–465. https://doi.org/10.1016/j.ijadhadh.2011.02.006
  7. Hart-Smith, L. J. (1982). Adhesive layer thickness and porosity criteria for bonded joints (AFWAL-TR-82-4172). Douglas Aircraft Company. https://apps.dtic.mil/sti/pdfs/ADA129817.pdf
  8. National Aeronautics and Space Administration [NASA]. (2016). NASA-STD-8739.1B with Change 2, Workmanship standard for polymeric application on electronic assemblies. https://standards.nasa.gov/sites/default/files/standards/NASA/B/2/nasa-std-87391B-Change-2.pdf
  9. Occupational Safety and Health Administration [OSHA]. (n.d.). Isocyanates. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/isocyanates
  10. Parker, B. M. (1983). The effect of composite prebond moisture on adhesive-bonded CFRP-CFRP joints. Composites, 14(3), 226–232. https://doi.org/10.1016/0010-4361(83)90008-3
  11. Szycher, M. (2012). Szycher's handbook of polyurethanes (2nd ed.). CRC Press. https://doi.org/10.1201/b12343

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.