BlogKaltec Voices
Same spec, different results.
- Type
- Kaltec Voices
- Published
- 24 November 2026
- Prepared by
- Jonghwan Moon
- Role
- Technical Staff
Each number on a data sheet comes from a test run at a set temperature, with set water and motion, for a set time, so hydraulic oils and greases with the same spec still part ways once they meet the condensed water, pellet dust and constant pressure swings of an injection molding machine. Read the test method behind each number to measure the gap between the lab and the machine, and where it is wide, only a re-test with that plant's own water, dust and operating conditions lets you judge the result in advance.
Background
In the middle of one rainy season, I opened the sample valve on a hydraulic tank at an injection molding plant to take a routine sample. The oil in the bottle was milky, and after it stood for a while a thin layer of water settled at the bottom. On the breather filter, where the tank breathes, pellet dust blown over from the granulator sat in a gray coat. That oil had been chosen for the water separability value on its data sheet.
The number was not wrong. It came from a test that stirs the oil with an equal volume of distilled water at 54°C for 5 minutes. The water in this tank was humid air that had condensed over several weeks on walls cooled overnight, and it had settled out together with the pellet dust. We changed the breather, drained the water from the tank bottom, then compared the candidate oils again under that plant's conditions before choosing.
Each number on a data sheet comes from a test run at a set temperature, with set water and motion, for a set time. Before comparing the size of the numbers, read at what temperature the test ran, with what mixed in, how and for how long, and you can see how far that number holds on your machine. On site, the first thing I measure is that distance between the lab and the machine.
Water in the lab, water condensed in the tank
Water separability stirs 40 mL of oil with 40 mL of distilled water at 54°C for 5 minutes, then records how long the two take to separate again and how much emulsion is left (ASTM International, 2021b). It tests whether a large amount of water entering at once separates quickly.
Condensed water is almost as clean as distilled water, but it gets in a different way. Each time the mold opens and closes, the cylinders draw oil out and send it back, so the tank level rises and falls and the tank breathes in that much outside air. Humid air turns to water on walls cooled overnight, and that water travels through the system for weeks, mixed into the oil in small amounts. The number closer to this condition is hydrolytic stability. Three parts oil and one part water go into a bottle with a copper strip and are rotated at 93°C for 48 hours, then the copper's weight change, the change in the oil's acid number and the acidity of the water layer are measured (ASTM International, 2021a). The rust test stirs 300 mL of oil with 30 mL of distilled water or synthetic seawater at 60°C with a steel specimen immersed, then checks the specimen for rust (ASTM International, 2025c). A spot like the tank wall above the oil level, never immersed and only collecting dew, is not part of this test.
If an oil cooler tube leaks, the story changes again. The water that enters then is cooling water carrying treatment chemicals and hardness, and no test run with distilled water or synthetic seawater has met that water. The oxidation life test adds water as well, but there it works with iron and copper catalysts while oxygen is bubbled through at 95°C, speeding the reaction until the acid number reaches 2.0 mg KOH/g (ASTM International, 2025b). When I receive the hydraulic oil change records for injection molding machines, the first thing I do is sort out whether each change was made for oxidation or for water and dust. How much weight oxidation life, the biggest number on the data sheet, carries on that machine, I only know after seeing that split.
No test adds dust
None of the tests on a data sheet is run with dust mixed in. The closest number is the cleanliness code, which records the count of particles of 4, 6 and 14 µm and larger in 1 mL of oil as three code numbers (ISO, 2021). But that code is measured on new oil, in the drum or at filling. The air the tank breathes in each time its level rises and falls carries pellet dust and moisture together. When the breather filter clogs or gets wet, it filters both less well, and unless the breather holds a desiccant, moisture passes almost straight through. The finer a valve's control of injection speed and pressure, the more sensitive it is to those particles.
Constant pressure swings and pins that almost stop
Pressure rises and falls with every shift between injection, holding and clamping, and when the mold opens, oil from the cylinders rushes back to the tank at once and drags air in with it. If the oil reaches the pump again before that air escapes, it shows up as noise and pressure fluctuation. The air release test blows compressed air into oil held at a set temperature of 25, 50 or 75°C, then times how long the entrained air takes to fall to 0.2% by volume (ASTM International, 2026). Even this value cannot rank oils for systems with small tanks, where the oil stays only briefly, so I use it only to narrow the candidates (ASTM International, 2026).
On a machine whose toggle link pins and bushings are greased, I look at the wear number. The wear value on a data sheet usually comes from the four-ball test, which runs four steel balls against each other in one direction for an hour at 75°C, 1,200 rpm and 392 N (ASTM International, 2023). A toggle pin swings through a wide angle as the mold opens and closes, but it takes the clamping force at the end position, where the link is nearly straight and the pin almost stops. Motion is smallest when load is largest, so no oil film forms, and the grease has hardly any time to flow back into the contact. A test closer to small motion under heavy load is the fretting wear test, which oscillates two thrust ball bearings quickly through a narrow arc of about 12 degrees and then weighs what the races have lost. It was made to judge damage to car wheel bearings during long-distance shipping, so it does not fit a toggle pin directly, but in its back-and-forth motion it is closer than the four-ball test (ASTM International, 2024). Pins and bushings slide rather than roll, so I also ask whether there is a value from a sliding oscillation test. That test presses a steel ball onto a test disc at 200 N and oscillates it over a 1 mm stroke, 50 times a second for two hours, measuring the friction coefficient and the wear scar on the ball, on an SRV machine named for the German initials for vibration, friction and wear (ASTM International, 2025a).
Putting it to work
Next time you choose a hydraulic oil or grease, set your machine's conditions beside the candidate's data sheet, one line at a time.
| Test | Lab condition | What to check |
|---|---|---|
| Water separability | Equal volume of distilled water, 54°C, 5 min stirring | How water gets in, breather condensation or cooler water |
| Hydrolytic stability | Three parts oil to one part water, copper, 93°C, 48 h | How long water stays in the oil, Karl Fischer water and acid number trends |
| Rust prevention | Distilled water or synthetic seawater, 60°C, immersed steel specimen | Rust on the tank wall above the oil and inside the lid |
| Oxidation life | Water and catalyst, 95°C, time to acid number 2.0 | Whether past changes were for oxidation or for water and dust |
| Cleanliness code | Particle counts at 4, 6 and 14 µm in new oil | Code of in-service tank samples, breather filter condition, desiccant or not |
| Air release | Time at a set temperature for entrained air to fall to 0.2% | Process steps where pressure wavers, tank volume and pump flow |
| Grease wear | Four-ball, one-way rotation for an hour | Load and motion on the pin at the clamping end position, sliding oscillation test values |
The farther the right column is from the middle one, the less the data sheet's ranking holds on that machine. The way to close that gap is not to look for a bigger number but to test the candidates again under that plant's conditions. Mix water drained from the tank bottom into each candidate oil and see which one separates first. Our technical team asks about the right column of this table first, puts candidates that pass the quick check into one or two machines that face that plant's water and dust as they are, and takes samples at set intervals. We record the results with the water, temperature and duration of each test, down to which number reversed under which condition.
Conclusion
A data sheet is still the fairest basis for comparing products. That fairness comes from putting every product in the same lab, and your machine is not in that lab. Read the test method behind a number and you see which conditions it speaks for; beyond them, it has to be measured again in your plant's water, dust and pressure.
The numbers on a data sheet have not yet met the water in your machine.
Sources
- ASTM International. (2021a). Standard test method for hydrolytic stability of hydraulic fluids, beverage bottle method (ASTM D2619-21). ASTM International.
- ASTM International. (2021b). Standard test method for water separability of petroleum oils and synthetic fluids (ASTM D1401-21). ASTM International.
- ASTM International. (2023). Standard test method for wear preventive characteristics of lubricating grease, four-ball method (ASTM D2266-23). ASTM International.
- ASTM International. (2024). Standard test method for fretting wear protection by lubricating greases (ASTM D4170-24). ASTM International.
- ASTM International. (2025a). Standard test method for measuring friction and wear properties of lubricating grease using a high-frequency, linear-oscillation (SRV) test machine (ASTM D5707-25). ASTM International.
- ASTM International. (2025b). Standard test method for oxidation characteristics of inhibited mineral oils (ASTM D943-25). ASTM International.
- ASTM International. (2025c). Standard test method for rust-preventing characteristics of inhibited mineral oil in the presence of water (ASTM D665-25). ASTM International.
- ASTM International. (2026). Standard test method for air release properties of hydrocarbon based oils (ASTM D3427-26). ASTM International.
- International Organization for Standardization [ISO]. (2021). Hydraulic fluid power, Fluids, Method for coding the level of contamination by solid particles (ISO 4406:2021).