KALTECKOREA

BlogKaltec Voices

What to do in the first two days of a claim

Type
Kaltec Voices
Published
24 November 2026
Prepared by
Jaemin Seo
Role
Technical Staff

When a quench oil hardness claim comes in, the first two days go to keeping traces before naming a cause: used oil samples, retained lot samples, paired good and bad parts, and tank records. A supplier that links those traces by lot number and sets them against the tank's past analyses turns a claim from an argument over causes into reading the same records together.

Background

The call about uneven hardness in heat-treated parts usually comes from the customer's quality lead. At outgoing inspection a few parts from one basket came in under spec, and on remeasuring, values differ from spot to spot even within one part. After hearing it all, my first question is not about the cause. "You haven't thrown anything out of the tank yet, have you?"

Oil is not the only thing that moves quench hardness. Even with the same oil, hardness drops if the few seconds from furnace to immersion run long. On the oil side alone, water, sludge from oxidation, tank temperature and agitation each leave a different trace. Most traces of oil and tank sit in the tank and in floor records, and they vanish in a day or two while the plant runs as usual. Whether a claim's cause can be found is decided by what was kept in the first two days. So I spend those two days guarding traces, not naming a cause.

Traces that routine work erases

Quench oil changes as it is used. Each hot part it takes pushes oxidation and thermal breakdown a little further, and the by-products settle unevenly on part surfaces as sludge. Cooling rates then differ from spot to spot, and hardness comes out uneven. Water causes trouble even in small amounts. Moisture in the oil brings soft spots, staining and cracks, and at worst fire (Totten et al., 1993). The guide for evaluating hydrocarbon-based quench oil also measures used oil viscosity, water, flash point and precipitation number, each by its own test method (ASTM International, 2021b).

The trouble is that ordinary steps after a claim wipe these traces out. A low level gets topped up with new oil, and water seen at the bottom gets drained. Filters are changed, and the tank is heated and agitation restarted to keep production going. Each step is right on its own. But a sample taken after a top-up is not the oil from the day of the defect, and a water reading after draining is not that day's value. Once, after the whole charge was replaced, the same defect came back and we looked for the first oil, but a waste oil hauler had already taken it, and we never could say whether it was the cause.

What to keep before restarting

After a traffic accident, the cars behind mean you cannot leave your car stopped for long, so before moving it you photograph where the wheels sit and the marks on the road. A quench line cannot stop for long either, because of the production schedule. So I do not ask to keep the line stopped. I ask to keep what must be kept first, before it runs again.

First, used oil samples. Before any top-up, with agitation running, take one in a clean, dry bottle from the sample valve on the circulation line or from mid-depth in the tank. Take a separate bottle from the bottom drain. Water and sludge settle to the bottom, so the two bottles read differently, and that difference is a trace too. Take hot oil wearing protective gloves and safety glasses, and cap the bottle at once to keep out moisture from the air. Write on the bottle the time and the tank temperature, and photograph the level gauge reading and the foam and color of the oil surface. The floor check of dropping a few drops on a hot plate and listening for crackle helps set a direction, but it leaves no number, so it cannot replace a lab sample.

If water turns up, find its way in the same day. Look for leaks on the cooling water side of the oil cooler, water on parts coming from the washer upstream, and condensation above the tank. Drain the water with the path still open, and it comes back.

Next, pairs of bad and good parts. Keep bad and good parts from the same load together, noting where each sat in the basket. If soft parts cluster in the middle or bottom of the basket, look at oil flow first. If they are scattered regardless of position, look at material and furnace together. Most hardness claims that reach me come from sealed batch furnaces. For a mesh belt continuous furnace, note the position across the belt width instead. Good parts stay with them because the baseline for comparison has to be in the same load.

Then, tank temperature and agitation records. Collect that day the temperature recorder chart, when the agitator or circulation pump stopped and restarted, agitator motor current, transfer time records from furnace to immersion, and recent maintenance history. The cooling curve test common in certificates and product specs is run on unagitated oil, and the standard itself states its results do not correlate with those in an agitated tank (ASTM International, 2021a). Even if the oil checks out in the lab, weak agitation in the tank makes the vapor film collapse at different times on each part, and hardness splits (Totten et al., 1993). Oil samples and agitation records must be kept the same day to match.

Two samples linked by lot number

If used oil samples show the tank now, retained samples of unused lots show the oil as it came in. We keep a sample of every lot shipped, and when a claim comes in, we pull that day the certificates and retained samples of the lots recently added to that tank. If unopened drums of the same lot remain in the customer's store, we mark them not to be used. Running new and used oil side by side in the same tests shows whether the product differed from the start or changed in use. If the retained sample's cooling curve and properties match the certificate or product spec but only the used oil's viscosity and precipitation number have risen sharply, I look first at oxidation in use. If the retained sample itself differs from the certificate or spec, I look first at how that lot was made. If both samples are normal, attention moves to the tank's agitation, the basket and the furnace. Some of that I do not know. The customer's heat treatment lead and the material supplier know furnace atmosphere and steel hardenability better than I do.

This is where lot number matching comes in. A quench tank is not filled from one lot. Over months, several lots are added on top of the first fill. So we match the dates and lot numbers in the top-up records against the date of the load where the defect first appeared. If defects began right after a certain top-up, look at that lot first. If they grew slowly regardless of top-ups, look first at oxidation or water. Check too whether the material heat number changed around the same time. Some claims had top-up records without lot numbers, and this matching could never be done.

Sometimes judging this sample's values takes just a day. That is when there is a record of regular used oil analysis for that tank. Knowing how water, viscosity and cooling curves moved across past analyses, you can say whether this value is inside or outside the tank's usual trend. Without that record, the one value can only be set against a spec sheet, and whether an in-spec value is normal for that tank stays unknown.

Putting it to work

In the first hours after the call, the job is less to stop work than to change its order. Put off top-ups, water draining and filter changes until samples are taken, and set aside that load's bad and good parts with their positions. When remeasuring hardness, measure where the decarburized surface layer has been removed, mark the spots, and collect the tempering furnace temperature records too. If tempering ran high, hardness comes out evenly low whatever the oil. If water turned up, drain it, top up the oil and repeat the hot plate check. If there is no crackle and the first load's hardness is normal, run the line as usual. If oil has already been drained, first check whether it is still in drums.

On the first evening, lay out what has been gathered on one line, in time order: the load where the defect first appeared, the top-up dates and lot numbers around it, temperature and agitation records, and the times samples were taken. In the report the quality lead sends up that day, write not the cause but what will be checked by when, and what to look at next depending on the results. The cause is written after test results come in, from day two on. A supplier that cannot produce those lots' certificates, retained samples and the tank's past analysis records by that evening leaves the cause to rest on this one sample.

On day two, run used oil and retained samples through the same tests, and check the bottom sample's water separately. Once the claim closes, put the retention period of each lot's retained samples and regular used oil analysis into the next contract terms. Then, on the first evening of the next claim, both are on the desk.

Conclusion

The cause of a quench hardness claim can usually be named only after test results come in. What those results can be set against is decided by the samples, parts and records kept in the first two days. Work with a supplier that links used oil and retained samples through the lot numbers in the top-up records and sets them beside the tank's past analyses, and a claim moves from arguing over blame to reading the same records together. The more plants keep tank analyses as a regular record, the more often the first day of a claim will be judged against past values instead of guesses.

My car still always carries a few clean, dry sample bottles, capped.

Sources

  • ASTM International. (2021a). ASTM D6200-21, Standard test method for determination of cooling characteristics of quench oils by cooling curve analysis. https://store.astm.org/d6200-21.html
  • ASTM International. (2021b). ASTM D6710-21, Standard guide for evaluation of hydrocarbon-based quench oil. https://store.astm.org/d6710-21.html
  • Totten, G. E., Bates, C. E., & Clinton, N. A. (1993). Handbook of quenchants and quenching technology. ASM International.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.