Black, hardened grease from an excavator swing bearing shows what a failure looks like, but the path to it differs with idle time, type of work, greasing intervals and seal condition. A failure analysis is finished only when that path has been traced back through operating conditions, greasing records and filter and seal replacement records.
Background
In my desk drawer is a lump of grease in a zip bag. I scraped it with a spatula from the raceway side after lifting the swing bearing seal on a 20-ton excavator. It went in as a light-colored grease with no molybdenum, and now it is black and hard and crumbles like chalk when pressed with a finger. Left overnight on filter paper, it spread almost no oil at the edges. It is a lump where the base oil has gone and only the thickener and something else remain.
That machine's failure was closed out by switching the grease to another product. A lump shows what state the grease ended in, but not the path it took to get there. The base oil may have run out before new grease arrived, dirt may have come in through a gap in the seal, or it may have hardened after mixing with a grease of a different nature. A different path means a different hand to stop the next failure. A failure analysis is finished only when the operating conditions and care that led the grease to that state have been confirmed. After an analysis that stops at a product name, the same lump turns up again in the same spot. So the first thing I ask on site is how the machine worked and how it was looked after once that grease went in.
What a failure looks like and the path to it
The international standard on reliability data for oil and gas equipment puts failure mode, failure mechanism and failure cause in separate fields (ISO, 2016). The standard on rolling bearing damage also records the appearance of damage apart from its causes (ISO, 2017). A worn raceway is the mode, the visible appearance, and black hardened grease is the evidence left beside it. In a swing bearing at least three mechanisms lead to the same appearance.
One is starvation. A swing bearing spends more time oscillating through small angles than rotating fast. Bearings oscillating through small angles usually run short of grease, and experiments show that the more base oil a grease releases, and the more freely it flows, the later early wear begins (Wandel et al., 2022). Grease that has given up all its base oil hardens to bare thickener, and if new grease cannot push it out, it turns black where it sits. Then the lump has no grit when rubbed between fingertips, and the raceway tends to show rows of wear marks spaced at the rolling element pitch.
Another is dirt and water. When the swing bearing's lip seal cracks or turns over, fine dirt mixes into the grease and makes an abrasive paste. This lump feels gritty at the fingertip, and a lab analysis shows high silicon.
The last is mixing. Put in a grease with a different thickener without pushing out enough of the old one, and it can soften or harden where they mix, and there is a separate test practice for evaluating mixtures of two greases (ASTM International, 2024). For any of the three mechanisms, the cause field can also hold a product defect or a selection that does not suit that spot, and if so, the side that supplied the grease should speak first. But the three paths end looking alike, so filling the cause field from the lump alone closes the analysis without asking which path it was.
Time the hour meter cannot count
To find what goes in the cause field, you first have to know how the machine worked. Greasing intervals are usually set by hour meter time, and the hour meter counts engine running time, which includes time with the bucket down and only the engine running. When one maker in North America gathered a year of telematics data from about 75,000 machines, idling averaged 38 percent. Another maker's representative said the ratio varies widely by site and job (Moore, 2020). The telematics data specification for construction equipment also has a field for cumulative idle hours, separate from cumulative operating hours (ISO, 2020).
So even with the same interval set by the hour meter, the work the machine did in between differs. A machine with little idling actually works longer within the same interval, and its grease runs out that much sooner. The greasing table in an operator's manual often has a separate line to shorten the interval for breaker or underwater work, but that line rarely makes it into the site greasing log.
The type of work also changes the shape of the swing. Loading dump trucks swings the upper structure widely, while digging a pipe trench on a narrow road oscillates a few degrees at a time in one spot. The more days of small-angle oscillation, the wider the path to starvation opens, and in such periods new grease reaches all the way round only if it goes in at several points while the upper structure is turned bit by bit. More grease does not settle it either. Pump it all into one spot and the lip seal gets pushed and lifts, and that gap opens a path for dirt. Watching whether old grease is pushed out evenly round the seal while greasing is the easiest way to judge the amount. The operator and the site manager know better than I do which work went on for how many days. For a machine without telematics, their daily work reports are all the record there is.
The baseline a product switch erases
The fix of switching products has a point. If the product was the cause, that ends it, and if the failure stops after the switch, it looks as if the cause was right. But on the day the grease is switched, other hands move too. Someone fits a new seal, greasing dates are moved up, and meanwhile the machine moves to another site. When a failure stops after the switch, it is not clear whether it was the new grease, the seal fitted around then or the change of work. And if the new grease went in without pushing out enough of the old, it opened a new path to mixing.
So even when the product is switched, I do not close the analysis, and I record the operating conditions and greasing method from before the switch as they were. Only with that record can you say what stayed the same when the same failure comes back.
Putting it to work
The excavator that gave me the lump in the drawer came back a few months after the grease switch with a clunk on swing, and the same-looking grease came out of the same spot. That time I went back past the switch date and reopened the records.
I put operating conditions first. From the telematics I pulled operating hours and idle hours by month for the half year before the failure, and next to them wrote the type of work from the daily work reports for the same months. The machine had spent four months on urban pipe work, and those four months had little idling and short swings.
Next to that I put the greasing records. Greasing dates by hour meter were all there, but there was no place to note how much went in each time or whether the upper structure was turned while greasing. Through the four months of pipe work, the greasing interval and method stayed the same as during truck loading. There was no field for the product name either, so whether another grease had gone in meanwhile I learned only by asking the operator. He said he always greased from the same tub. The day the path to mixing opened widest was the day the product was switched. The service record noted that on that day the grease was pumped in while turning the upper structure until new grease color showed all round the seal, and the four months of pipe work came after.
Last, I looked at the filter and seal replacement records. Find the days the swing bearing seal and bushings were replaced and, if there is an auto-lube unit, the days its inlet filter was opened, and check whether months of wet or muddy work fell in between. That machine had no record of a seal change since the seal lifted at the first failure was refitted. The grease from the second failure did not show high silicon on analysis, and the lip lifted the second time had no cracks or turned-over spots. So I judged dirt entry unlikely. What remained were the four months of small swings and the grease put in at the same interval and by the same method all through them. That case was closed not by switching the grease again but by tying the greasing interval and method to the type of work.
When the next failure report is about to close with a product switch, cut these three records to the same period before the failure and lay them side by side before placing the order. Only when the side that supplied the grease also sits at that table and reads the three records together does the analysis go past the product name, back to the operating conditions before the failure.
Conclusion
A failure analysis that stops at a product name does not change the date of the next failure. Whether the grease starved, took in dirt or mixed is sorted out only when operating conditions, greasing records and filter and seal replacement records are set on the same period. The operating conditions and greasing method of a case sorted out that way stay on as that site's record, a starting point for pinning down what changed when the same lump comes out again.
A site that keeps records adds a baseline with every failure, and a site that only switches product names adds only names to suspect. A field for idle hours is already in the telematics data specification. The newer the machine, the more idle time is logged separately and the easier operating conditions are to fill in, so I expect the gap between the two kinds of site to widen faster.
The lump in the drawer says only that the grease hardened. Why it hardened is told by the four months of records that machine left.
Sources
- ASTM International. (2024). ASTM D6185-24, Standard practice for evaluating compatibility of binary mixtures of lubricating greases. https://store.astm.org/d6185-24.html
- ISO. (2016). ISO 14224:2016, Petroleum, petrochemical and natural gas industries — Collection and exchange of reliability and maintenance data for equipment. https://www.iso.org/standard/64076.html
- ISO. (2017). ISO 15243:2017, Rolling bearings — Damage and failures — Terms, characteristics and causes. https://www.iso.org/standard/59619.html
- ISO. (2020). ISO/TS 15143-3:2020, Earth-moving machinery and mobile road construction machinery — Worksite data exchange — Part 3: Telematics data. https://www.iso.org/standard/76394.html
- Moore, W. (2020, March 24). How to manage engine idling for efficiency. Construction Equipment. https://constructionequipment.com/how-manage-engine-idling-efficiency
- Wandel, S., Bader, N., Glodowski, J., Lehnhardt, B., Leckner, J., Schwack, F., & Poll, G. (2022). Starvation and re-lubrication in oscillating bearings: Influence of grease parameters. Tribology Letters, 70, 114. https://doi.org/10.1007/s11249-022-01655-7