Applying a thicker coat or switching to another coating is the usual response when parts still scale and decarburise under an anti-scale coating, but a coating works only by blocking oxygen's path to the steel, so unless the place where that path opened is found, the same result keeps coming back. What actually lies behind it can be the wrong film thickness, an undried film, heating outside the coating's rated range, a dirty substrate before coating or overlong heating, and sometimes two or more at once.

Background

A tool steel block is coated carefully with anti-scale coating and put in the furnace, yet when it comes out, thick black scale sits under the spots where the coating lifted or cracked. A cross-section shows a carbon-depleted layer just under the surface as well. The material lost as scale is gone, the decarburised layer does not harden properly on quenching and must be ground off, and parts with no allowance left to grind are simply rejected. Scale and decarburisation during heating are both counted as losses that cut steel yield (Torkar et al., 2007).

Heating steel in air grows iron oxide scale on the surface. Above 700 °C, iron forms a three-layer scale of haematite, magnetite and wüstite from the outside in, following the parabolic law: fast at first, then slower with time (Chen & Yuen, 2003). In the same heating, carbon at the surface reacts with oxygen or water vapour and leaves, and a ferrite layer forms on the carbon-depleted surface. Scale and decarburised layer grow together, and how they behave depends on the temperature region the steel sits in (Choi & van der Zwaag, 2012).

An anti-scale coating works by blocking oxygen's path to the steel surface. Components such as silica and alumina form a layer during heating that lets little oxygen through even at high temperature, and that layer reduces both scale and decarburisation (Torkar et al., 2007). So if scale and decarburisation appear despite the coating, either the film did not close that path completely or the conditions went beyond what the film could stand.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph the coating as applied and as it came out of the furnace, record film thickness, drying time and conditions, furnace temperature and hold time, and compare them with the coating's technical data sheet, the TDS, and the heat treatment instruction.

Hypothesis 1: wrong film thickness

The film tends to end up thin when it is brushed on by hand, on shapes where it thins easily such as edges and chamfers, and when the coating has been thinned heavily or sprayed from too far away. Build it up in one heavy pass, on the other hand, and it ends up thick. Watch a large die block being brushed: the broad faces get a generous coat, while at the edges the brush only skims past and the substrate shows through. After heat treatment the block has a band of scale along the edges, and a net of cracks runs across the middle of the heavily coated face.

To block oxygen, the film has to form an unbroken layer during heating. In a glass coating, the molten glass layer acts as a barrier to oxygen diffusing in, and in a glass-ceramic coating the amorphous part fills in by viscous flow to give a dense film (Liu et al., 2011; Yu et al., 2021). Where the film is thin there is too little material to fill in, so substrate shows through or holes remain. A thick film brings a different problem. A liquid film of dispersed particles cracks above a certain thickness because of capillary stress as it dries (Singh & Tirumkudulu, 2007), and those cracks become channels for oxygen to reach the substrate during heating. A study comparing coatings for heating before forging also found that decarburisation varied with the substance applied and its concentration (Widomski et al., 2021).

Thickness is simply a matter of measuring. While coating, use a wet film gauge, and once dry, a magnetic film thickness gauge, measuring broad faces, edges and the areas around holes separately and comparing them with the TDS recommended thickness. Check the dry film with a magnifier for cracks before it goes into the furnace, and after heat treatment note whether the scale gathered at the edges or followed cracks in the thick areas.

If thickness looks like the cause, build the film in several thin coats instead of one heavy one, drying each for as long as the TDS specifies. Give edges and chamfers an extra stripe coat first, and if hand brushing is uneven, consider switching to spray. Write the dilution ratio and spray distance into the work standard as numbers so the same film comes out whoever applies it.

Hypothesis 2: undried film

Suspect this when a water-based coating is applied and the part is loaded at once, on days when drying is slow, as in the rainy season or winter, and when a thick coat has dried on the outside while staying wet inside. Suppose that on a humid day, pressed by the furnace schedule, a freshly coated part is checked only by touching it to see that the outside is dry, and is loaded as it is. When it comes out, the coating has small blisters and burst marks here and there, with scale underneath.

An undried film causes trouble in two ways. One is the drying itself. A film can crack under capillary stress as it dries (Singh & Tirumkudulu, 2007), and if it dries in a hurry inside the furnace, those cracks form before the film has densified and can remain as paths for oxygen. The other is water vapour. Water in the film comes off as vapour right above the steel surface early in heating, and water vapour has long been treated as a factor that markedly changes the high-temperature oxidation behaviour of metals and alloys (Saunders et al., 2008). In a study that heated spring steel in a range of atmospheres, a preformed oxide scale protected against decarburisation only in dry oxygen-containing gas, and not when water vapour was present (Chen et al., 2020).

Check by weight, not by fingertip. Leave a coupon coated with the same product under working conditions and weigh it at intervals; the point where it stops losing weight gives the drying time actually needed. Find in the work records the time between coating and loading and the temperature and humidity that day, compare them with the TDS drying conditions, and look for blisters and burst marks in the coating on parts that have come out.

With the cause narrowed to an undried film, manage drying by set conditions and times rather than by touch. Keep to the TDS drying conditions, and set aside a warm-air drying spot for humid or cold days. If a thick film is needed, apply it in thin coats with drying in between so it dries right through. A minimum drying time between coating and loading, written into the furnace schedule, holds even on busy days.

Hypothesis 3: out of rated range

Each coating has its own temperature range in which the film does its job. Think of this hypothesis when one coating is used across steel grades heated to different temperatures, when a coating meant for forging temperatures is moved to lower hardening temperatures, and, the other way round, when a low-temperature coating is taken higher. There are days when a coating used for forging heats is applied unchanged to parts hardened at a lower temperature. The coating on the parts that come out crumbles away like powder, and the surface beneath shows scale and a decarburised layer.

The film densifies only once the temperature reaches a certain level. In a study of a glass-ceramic coating, the film still had surface pores at 800 °C and 900 °C, and visible pores disappeared only at 1000 °C. The same study points out that glass coatings melting below 800 °C suit only some special steels heated to low temperatures, and that glass components can react with the substrate at high temperature and cause surface quality problems (Yu et al., 2021). The effect of a silica and alumina based coating was likewise greatest at 1000 to 1200 °C (Torkar et al., 2007). It also matters that the temperature band where the film has not yet densified can overlap the band where decarburisation runs most readily. In one spring steel study, the tendency to decarburise was greatest at 800 °C and fell at 1000 °C, where a ferrite layer could not form (Chen et al., 2020).

Set the operating range on the TDS beside the heating temperature in the heat treatment instruction. Look not only at the hold temperature but also at the bands passed through during heat-up and how long the part stays in them. If possible, fix a thermocouple to a part to measure its real temperature, and note whether the coating comes out powdery, fused smooth like glass, or fused to the substrate and hard to remove; that suggests which side of the range was missed.

If the range was indeed missed, the answer is a coating whose range covers that process temperature. Where heating temperatures differ widely between steel grades, do not standardise on one coating; split them by temperature band. If the heat-up plan lingers in the band before the film densifies, review with the furnace and coating suppliers how to pass through it faster.

Hypothesis 4: dirty substrate

Look this way when coating goes onto a surface with cutting fluid or rust preventive left on it, onto rust and scale from an earlier heat treatment or from storage that was not fully removed, onto spots touched with bare hands, or onto a surface still wet from washing. Think of parts sprayed with rust preventive after machining and coated straight away, without degreasing, on a busy day. The coating beads up on the surface so the substrate shows through in places, and after heat treatment spots of scale follow those places.

A coating forms an unbroken film only when it wets and bonds evenly to the substrate. An oil film repels water, and there is a standard test that detects hydrophobic contamination by whether a sheet of water breaks up on the surface; it is used to control processes for removing such contaminants (ASTM International, 2021b). In a study of epoxy paints on contaminated steel, engine oil and silicone oil lowered adhesion, corrosion products left after light abrasive cleaning caused the largest loss at 70 to 90%, and on contaminated substrates the film mostly failed at the interface (Moshkriz et al., 2026). That result is not about heat-treatment coatings directly, but a film applied over rust and leftover scale can be expected to bond poorly for the same reason. Scale also develops cracks and pores that give oxygen a path to the metal surface (Torkar et al., 2007), so a coating on top of it does not wrap the steel itself.

Before coating, splash water on the surface to see whether it spreads as an even sheet or breaks into beads. Wipe with a white cloth to see whether oil comes off, and look for rust or dark scale marks left behind. If the coating crawls or opens up in pinholes while being applied, photograph those spots and match them against the scale spots after heat treatment. Find in the work records when and how degreasing and rust removal were done.

If a dirty substrate is the cause, fix surface preparation as a set process step. Remove oil with a degreaser, take off rust and old scale by blasting or pickling, and dry fully. Coat prepared parts promptly rather than leaving them standing, and have handlers wear gloves. Putting the water-sheet check into the work standard before coating also catches faults in the degreasing process early.

Hypothesis 5: overlong heating

This applies when hold times are set long to heat large sections through, when parts wait at temperature in the furnace because of equipment trouble or schedule delays, and when one part is reheated several times. One Friday afternoon, a load stayed in the furnace several hours longer than planned because of an equipment check. With the same coating at the same thickness, that batch alone shows thicker scale and a deeper decarburised layer than usual.

A coating slows oxidation but cannot stop it altogether. The reduction in scale loss from a silica and alumina based coating was 30 to 60%, depending on heating time and temperature and on steel grade (Torkar et al., 2007). In a test that heated glass-coated stainless steel at 1250 °C for 9 hours, weight gain fell by 91.7% but did not vanish (Liu et al., 2011). The oxidation that remains keeps adding up over time, and decarburised depth and scale thickness both grow with heating temperature and time (Choi & van der Zwaag, 2012). So with the same film, longer heating lets more oxygen through in total, and scale and decarburisation appear under a coating that is normally trouble-free.

Find in the furnace records how long that batch actually stayed at temperature and compare it with the instruction. Section one part each from a normal batch and the long batch and measure the decarburised depth, which puts a number on the effect of time; the depth is found by the standard methods of viewing the section under a microscope or by a microhardness traverse in from the surface (ASTM International, 2021a). For reheated parts, also look up in the history how many times they were heated.

Once long heating is confirmed, cut the hold to what the instruction requires, and set a procedure to drop to a lower waiting temperature when equipment stops, so parts do not sit at temperature. Record reheats and control their number. Where a process truly needs long heating, review with the supplier a coating or protective atmosphere that stands up to that time, and confirm with design whether the drawing leaves machining allowance to remove decarburisation.

Finding the cause

Even with five hypotheses, the first tools are the records and the eye. Coating and loading times, film thickness, furnace temperature and hold time are already on record or can be measured at once, and the shape of the coating as it comes out only needs a look before it is thrown away. Sectioning specimens to measure decarburised depth comes after that.

Where the scale formed is the biggest clue. Scale in bands along edges and chamfers or following cracks in thick areas points to film thickness, and scale gathered under blisters and burst marks points to an undried film. Spots that follow places where the coating beaded up, or follow handprints, point to a dirty substrate, while a coating that crumbles like powder or is fused to the substrate over the whole part points to the temperature range. If the coating looks sound but scale and decarburisation have deepened evenly in one batch only, look first at heating time.

If that still does not settle it, run control trials with small specimens of the same steel. Put specimens that differ only in thickness, fully dried against underdried, and degreased against not degreased into the same load, and compare scale and decarburised depth afterwards. Change only one thing at a time, or there is no telling what made the difference. An uncoated specimen in the same load also shows how much scale the coating saved in that run.

The final check is to heat-treat real parts again under the corrected conditions and measure decarburised depth at set locations by the same method. Only the same locations and the same method as before the change make a fair comparison. The job is done when the depth is back within the drawing's limit and stays there for several batches.

The hypotheses can overlap. A film laid on thick in one pass easily stays wet inside, so thickness and moisture become a problem together, and a film on a dirty substrate shows its weak points more the longer heating runs. In such cases, correct what is cheap and quick to fix first, surface preparation and drying, then thickness, and finally the temperature range and heating time, because while the first ones are unsettled the effect of changing the coating cannot be compared fairly either.

Limits and cautions

Film thickness, drying conditions and operating temperature range differ from one coating to another, so numeric decisions follow the product's TDS, and allowable decarburised depth and machining allowance follow the drawing and the customer specification. Judging decarburised depth is laboratory work done by a set method, and for parts where surface hardness and fatigue life matter, such as springs and tools, do not release on floor judgement alone; get the quality engineer to confirm. Where conditions are beyond what a coating can handle, review other methods such as protective atmosphere or vacuum heat treatment with the heat treatment supplier.

Safety matters too. When mixing and spraying coating, provide protective equipment and ventilation as set out in the product's safety data sheet, the SDS, and wear respiratory protection where powder becomes airborne. Early in heating, reactions occur as the coating's binder breaks down (Torkar et al., 2007), so extract smoke and fumes around the furnace by ventilation. Wear heat-resistant gloves and eye protection when loading and unloading coated parts, and clear spent coating and scale only once they have cooled.

Sources

  1. ASTM International. (2021a). ASTM E1077-14(2021), Standard test methods for estimating the depth of decarburization of steel specimens. https://store.astm.org/e1077-14r21.html
  2. ASTM International. (2021b). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  3. Chen, R. Y., & Yuen, W. Y. D. (2003). Review of the high-temperature oxidation of iron and carbon steels in air or oxygen. Oxidation of Metals, 59(5–6), 433–468. https://doi.org/10.1023/A:1023685905159
  4. Chen, Y. R., Xu, X., & Liu, Y. (2020). Decarburization of 60Si2MnA in atmospheres containing different levels of oxygen, water vapour and carbon dioxide at 700–1000 °C. Oxidation of Metals, 93(1–2), 105–129. https://doi.org/10.1007/s11085-019-09949-3
  5. Choi, S., & van der Zwaag, S. (2012). Prediction of decarburized ferrite depth of hypoeutectoid steel with simultaneous oxidation. ISIJ International, 52(4), 549–558. https://doi.org/10.2355/isijinternational.52.549
  6. Liu, P., Wei, L., Zhou, X., Ye, S., & Chen, Y. (2011). A glass-based protective coating on stainless steel for slab reheating application. Journal of Coatings Technology and Research, 8(1), 149–152. https://doi.org/10.1007/s11998-010-9302-1
  7. Moshkriz, A., Ekbrant, B. E. F., & Kiil, S. (2026). Adhesion investigation of waterborne and solventborne epoxy coatings on oil-contaminated and surface-corroded steel substrates. Progress in Organic Coatings, 221, 110534. https://doi.org/10.1016/j.porgcoat.2026.110534
  8. Saunders, S. R. J., Monteiro, M., & Rizzo, F. (2008). The oxidation behaviour of metals and alloys at high temperatures in atmospheres containing water vapour: A review. Progress in Materials Science, 53(5), 775–837. https://doi.org/10.1016/j.pmatsci.2007.11.001
  9. Singh, K. B., & Tirumkudulu, M. S. (2007). Cracking in drying colloidal films. Physical Review Letters, 98(21), 218302. https://doi.org/10.1103/PhysRevLett.98.218302
  10. Torkar, M., Uršič, V., Vode, F., & Lamut, M. (2007). The application of waste silica cyclone powder for the protective coating of steel billets. Metalurgija, 46(3), 161–164. https://hrcak.srce.hr/en/clanak/18354
  11. Widomski, P., Zwierzchowski, M., Barełkowski, A., & Tympalski, M. (2021). Case study of the effect of precoating on the decarburization of the surface layer of forged parts during the hot die forging process. Materials, 14(2), 422. https://doi.org/10.3390/ma14020422
  12. Yu, B., Du, Y., Wei, L., Zhang, X., Zuo, G., Wang, Y., & Ye, S. (2021). Valorization of coal gangue and vanadium-titanium slag into glass-ceramic coating for oxidation resistance of 60Si2Mn spring steel at high temperature. ISIJ International, 61(1), 326–334. https://doi.org/10.2355/isijinternational.ISIJINT-2020-008

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.