KALTECKOREA

BlogApplication notes

Why does the joint corrode around anti-seize coated bolts?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Special Purpose

It is easy to assume anti-seize also stops corrosion and to put the same compound on every bolt, but the metal powders and other ingredients in it can take part in corrosion, depending on the metals they touch and the surroundings. What actually lies behind it can be a galvanic couple between copper or graphite and aluminium or stainless steel, stress corrosion cracking from sulphur and halogens, moisture held in the crevice, or a compound that does not suit the material, and sometimes two or more at once.

Background

On maintenance day the cover bolts come out and the aluminium around the bolt holes is pitted and shedding white powder. On another machine there are brown stains and pinhole marks under the heads of stainless steel bolts, and the threads still carry the anti-seize applied at assembly. A pitted housing needs its holes remachined or the part replaced, and when bolts corrode and the joint loosens, leaks follow. If a crack grows into the bolt it can break in service, which makes it a safety matter.

Anti-seize is oil or grease loaded with solid powders such as copper, nickel, graphite or molybdenum disulphide, so that threads do not seize and can be undone later. One metal-loaded compound, even after its oil boils off at high temperature, leaves oxides of nickel, copper and zinc between the threads so the bolt can still come out (Barrett, 1990). Because these solids outlast the oil, the metals they touch decide whether corrosion follows. When two different metals are electrically connected and an electrolyte such as water, condensation or salt bridges them, the less noble metal becomes the anode and corrodes first; this is galvanic corrosion. The larger the potential difference between the two metals, the stronger the drive (NIH, 2026).

Bolts have another route as well. A tightened bolt carries a pulling force, tensile stress, for as long as it stays tight. When a part under tensile stress sits in a corrosive environment, cracks grow from small pits or flaws made by corrosion, and even a ductile part can break at a stress far below its yield strength; this is stress corrosion cracking (Barrett, 1990). So corrosion around anti-seize coated bolts shows up in two ways: metal wasting away, or cracks running into the bolt.

In such cases the technical team sets up the four hypotheses below and rules them out one by one. The start is always the same: photograph the corrosion before the bolt comes out, note which metal has corroded, then check the solids and service limits of the compound used in its safety data sheet, the SDS, and technical data sheet, the TDS, and compare them with the materials of bolt, nut and parent part and with the service environment.

Hypothesis 1: galvanic couple

Consider this hypothesis first where aluminium housings, covers or brackets are fastened with steel or stainless bolts coated with a copper-loaded compound, and where a graphite-rich compound is used on stainless bolts and flanges. Outdoor equipment reached by rain or washdown water and sites exposed to sea air make it more likely. Picture an aluminium cover beside an outdoor pump, held by stainless bolts coated with copper-coloured anti-seize. At maintenance a few months later the bolts are clean, but only the aluminium around the bolt holes has swollen with white powder.

In the galvanic series, which lists metals in order of potential, aluminium alloys sit at the active end where corrosion comes easily, copper sits on the more noble side, and graphite lies near the noble end (Barrett, 1990). When copper powder or graphite from the compound touches aluminium and moisture bridges them, the aluminium becomes the anode and corrodes. The series ranks corrosion potentials measured in a given environment, and the further apart two metals lie, the greater the drive, though the actual amount of corrosion does not always follow (ASTM International, 2021). The area ratio matters as well. In salt solution tests on aluminium alloys, galvanic current did not depend on the anode area but rose in proportion to the cathode area (Mansfeld & Kenkel, 1975). A film of copper powder spread widely over threads and bearing face can act as just such a large cathode, and its current falls on the narrow ring of aluminium around the hole.

Stainless steel behaves a little differently. Its thin passive film makes it act like a noble metal, but when that film breaks down inside a crevice it turns active and can corrode, depending on what it is coupled to (NPL, 2000). The space under a bolt head and between engaged threads is exactly such a crevice. In seawater tests with graphite composite couples, 316 stainless steel and Monel went from no corrosion to crevice corrosion and pitting, the small round pits seen on the surface (Tucker et al., 1990). Guidance from a stainless steel association also notes that graphite used in large quantities can cause galvanic corrosion of stainless steel (ASSDA, n.d.).

Start with what has corroded. If the aluminium is pitted and white powder has built up, the aluminium was the anode; brown stains and pinholes under stainless bolt heads or on flange bearing faces point to a passive film that broke down in the crevice. Measure with an ohmmeter whether bolt and parent part are electrically connected, and compare with joints on the same equipment that were made without anti-seize or with another compound. Check the solids in the compound used on its SDS.

If a galvanic couple is the likely cause, work through the ways of breaking it in order. First see whether metals of the same family can be used; if not, break the electrical path with insulating washers and sleeves, and if that is not practical either, put a barrier coating on both parts (NIH, 2026). Jointing compounds such as anti-seize do not normally provide electrical insulation, so do not rely on the compound for it, and where insulation has been fitted, measure again after installation that the path really is broken (NPL, 2000). Keep copper- and graphite-bearing compounds off aluminium, and measure the depth of pitting on housings already attacked to review strength and sealing again.

Hypothesis 2: sulphur, halogen cracks

Suspect cracking where crack-sensitive materials, such as high-strength studs, flanges on hot steam lines and pressure vessels, or stainless bolts, were assembled with a compound containing molybdenum disulphide or halogens, elements such as chlorine and fluorine. Coastal plant, joints under insulation and places reached by chlorine-based cleaners belong here too. Suppose studs pulled from a steam line flange at a routine inspection show hairline cracks at a few thread roots, and the remaining compound has turned black and hard. There is hardly any visible wastage on the surface.

Stress corrosion cracking needs tensile stress, a corrosive environment and a susceptible material together, and the higher the heat-treatment temperature and the lower the ductility, the more susceptible the material (Barrett, 1990). Of these, the compound can change the environment. In a bulletin on bolt degradation, the US Nuclear Regulatory Commission pointed out that molybdenum disulphide can decompose under high temperature and moisture and release sulphide, which promotes stress corrosion cracking. The same bulletin noted that chlorine, fluorine and sulphur can leach from sealants injected to stop leaks (NRC, 1982). Later bolting guidance for nuclear plants treated molybdenum disulphide as a lubricant that can contribute to stress corrosion cracking and said not to use it, and put high-strength bolts with an actual yield strength of 1,034 MPa or more under watch for cracking (NRC, 2010).

For stainless bolts, chloride needs a separate look. A report for the UK Health and Safety Executive found that most reported cases of chloride stress corrosion cracking in austenitic stainless steel occurred at 60 °C or above, but a significant number occurred below that. Those cases came with other conditions, such as chloride-rich layers built up by evaporation or deposition, and pitting or crevice corrosion already present (Parrott & Pitts, 2011). The space under a bolt head and in the thread gap is a place where water can seep in and dry out again and again, and halogens carried in a compound or a cleaner can stay behind there too.

Checking starts with pulling the bolt and examining the thread roots and the neck under the head with a magnifier, and suspect bolts get an inspection that reveals surface cracks, such as dye penetrant testing. Code-specified ultrasonic testing on its own has been judged not sensitive enough to catch cracking in its early stage (NRC, 1982), so send broken or cracked bolts to a laboratory to analyse the fracture face and the corrosion products for sulphur and chlorine. Check the sulphur, chlorine and fluorine content of the compound used in its SDS and lot certificate. Once cracking is confirmed, replace every bolt in the same conditions, keep compounds containing molybdenum disulphide or halogens off high-strength, high-temperature and stainless bolts, and buy low-sulphur, low-halogen grades with certificates. On plant with rules on lubricant content, such as nuclear plant, those rules come first (NRC, 2010).

Hypothesis 3: trapped moisture

Moisture is the condition under which the corrosion described above proceeds. Equipment washed down daily, pipes and pumps carrying cold water or refrigerant that sweat on the outside, outdoor structures in the rain and coastal plant in sea air all belong here. So do joints where washdown water has rinsed the compound away, leaving bare metal and loose solids. A chilled water flange in the rainy season is such a place. Condensation forms on the cold pipe and runs down, and a ring of water stain sits around the washer under each bolt head. A dry indoor line with the same bolts and compound shows nothing.

A galvanic couple does no harm just because the metals touch; current flows only when an electrolyte joins them. Moisture is that electrolyte, and the more ions such as salts or acids it carries and the better it conducts, the more severe the attack, while in poorly conducting water the attack tends to stay close to the junction (NPL, 2000). The corrosivity class of an atmosphere for metals is likewise set from how long surfaces stay wet, how much chloride is deposited and how much sulphur dioxide is in the air (ISO, 2012). The compound's ingredients change with moisture too. In friction tests with molybdenum disulphide powder at high humidity, the powder did not adhere well to steel, so more metal touched metal, and acids formed where moisture met molybdenum disulphide corroded the steel specimens (Peterson & Johnson, 1953).

See whether corrosion marks cluster on the low side where water collects or runs down, or on the side washdown water reaches. Comparing wet and dry locations that use the same bolts and the same compound shows how much moisture contributes. Find the seasons and times when condensation forms and the washdown schedule and cleaner type in the records, and when the bolt comes out, check whether the compound is still there or has been washed away, leaving bare metal and dry powder. Check the cleaner's SDS for chloride.

When moisture turns out to be the main condition, start by removing places where water can sit. Provide a drainage path, repair the insulation and vapour barrier on sweating lines, and cover bolt heads and nuts with protective caps or sealant. For equipment that is washed down, consider switching to a low-chloride cleaner, and where the compound washes away, set a reapplication interval and put it in the maintenance plan. Reducing moisture slows both galvanic corrosion and stress corrosion cracking, so it is worth doing first even when other causes overlap.

Hypothesis 4: wrong compound type

Where the store holds a single tin of anti-seize and it goes on carbon steel, stainless and aluminium bolts alike, suspect the choice of compound first. It is the same when a compound bought for hot exhaust flanges ends up on aluminium covers, or when carbon steel bolts are replaced with stainless ones and the compound stays the same. On the workbench a large tin of copper-coloured anti-seize has a brush standing in it, and that brush passes in turn over an exhaust flange, a stainless instrument tubing fitting and the bolts of an aluminium cover.

Each compound suits particular materials and temperatures, depending on its solids. Stainless steel association guidance says compounds based mainly on nickel suit high temperatures better, and that graphite in large quantities can cause galvanic corrosion of stainless steel, against which nickel plating has been used (ASSDA, n.d.). NASA fastener design guidance says not to use a silver-bearing compound on aluminium or magnesium parts, and in the galvanic series of the same document nickel too sits on the more noble side of aluminium (Barrett, 1990). Nickel-based compounds suit stainless steel and heat, but they still differ in potential from aluminium, so for aluminium or magnesium a metal-free, non-metallic compound is the choice that forms no couple. Which metal pairings are acceptable is judged against an established reference, such as the US Department of Defense standard on galvanic compatibility (DoD, 2021).

The first check is to pull out the equipment list. For each corroded joint, write down the materials of bolt, nut, washer and parent part together with the compound used there, and hold each pairing against the galvanic compatibility reference and the recommended materials and service temperature in the TDS. Where the ingredient declaration is vague, ask the supplier for the solids and the sulphur and halogen content. Confirm with the fitters as well whether the work instruction names a compound and what was actually applied on the floor.

Once an unsuitable compound is confirmed, set the compound to use for each material. Specify a metal-free compound for aluminium and magnesium, a nickel-based compound for hot joints in stainless steel and nickel alloys, and a grade that meets the rules on plant with content requirements, then label each tin with its materials and store them apart. Writing the product name into work instructions and the bolting standard means the compound changes along with the bolt. Clean joints already done with the wrong compound at the next maintenance and apply the right one.

Finding the cause

Four hypotheses do not mean four separate investigations. Rule them out one at a time, starting with what is easy to check. Which metal corroded, what the compound contains and what the bolt and parent part are made of can be learnt by undoing one bolt and reading the paperwork, and moisture shows up on one walk round the site. Cracks and chemical analysis need a laboratory, so they come next.

The first clue is the form of the corrosion. If the aluminium parent part is pitted around the bolt holes with white powder built up, suspect a galvanic couple between copper or graphite and aluminium first. Brown stains and pinholes under stainless bolt heads or inside the bearing face point to a passive film that broke down in the crevice, and to graphite. If the surface looks sound but there are cracks at the thread roots, or a bolt has broken, suspect stress corrosion cracking brought on by sulphur and halogens.

Next is the difference between locations. If, among joints with the same materials and compound, only the wet ones corrode, moisture is the dividing line; if the environment is the same but only certain material pairings corrode, look at compound choice and galvanic couples. If that still does not settle it, run a control trial. At the same location, refit a few bolts with a metal-free compound or with insulating washers, leave the rest as they are, and compare them at the next maintenance. Change only one thing at a time, or there is no telling what worked.

The final check belongs to the laboratory. For a cracked bolt, examine the fracture face and a section to see where the crack started and how it grew, and look for sulphur and chlorine in the corrosion products. Confirm the sulphur and halogen content of the compound and the cleaner by analysis or from supplier certificates. Only with these results can it be decided whether to replace other bolts in the same conditions and how far to widen the inspection.

The hypotheses often overlap. Galvanic corrosion needs metals in contact and an electrolyte (Barrett, 1990), so a couple between copper powder and aluminium only causes corrosion where there is moisture. Chloride built up in a crevice both breaks down the passive film on stainless steel and sets up the conditions for stress corrosion, and an unsuitable compound is where all of this starts. In such cases, reduce moisture and switch to a compound that suits the material first, then look again at whatever corrosion or cracking remains.

Limits and cautions

Service temperature, suitable materials and sulphur and halogen content differ by compound, so numeric limits follow the product's TDS and certificates, and on plant with rules on bolts and lubricants, such as nuclear plant, pressure vessels or high-temperature piping, those rules and the inspection body's judgement come first. Do not reuse a bolt suspected of cracking; replace it, and leave the cause of cracking and the soundness of the remaining bolts to a materials laboratory and the plant engineer. Whether a pitted housing or flange stays in service is for the design engineer to decide against its design strength and sealing needs.

Safety matters too. Follow the SDS for the compound and cleaner, wear gloves and eye protection, and keep metal-loaded compounds off skin and out of eyes. Corroded or cracked bolts can be weaker than expected, so loosen or replace bolts on pressure equipment only after pressure and temperature have been removed and the equipment is locked out, and do not undo many at once.

Sources

  1. ASTM International. (2021). ASTM G82-98(2021)e1, Standard guide for development and use of a galvanic series for predicting galvanic corrosion performance. https://store.astm.org/g0082-98r21e01.html
  2. Australian Stainless Steel Development Association [ASSDA]. (n.d.). Technical FAQ 5: Galling and its control. Retrieved November 2026. https://assda.asn.au/publications/technical-faqs/galling-and-its-control
  3. Barrett, R. T. (1990). Fastener design manual (NASA Reference Publication 1228). NASA Lewis Research Center. https://ntrs.nasa.gov/citations/19900009424
  4. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation.
  5. Mansfeld, F., & Kenkel, J. V. (1975). Galvanic corrosion of Al alloys—III. The effect of area ratio. Corrosion Science, 15(4), 239–250. https://doi.org/10.1016/S0010-938X(75)80019-9
  6. National Institutes of Health, Office of Research Facilities [NIH]. (2026). Galvanic corrosion in design and construction (Technical Bulletin, Issue 161). https://orf.od.nih.gov/TechnicalResources/Documents/Technical%20Bulletins/26TB/Galvanic%20Corrosion%20in%20Design%20and%20Construction%20-%20June%202026%20TB_508.pdf
  7. National Physical Laboratory [NPL]. (2000). Guides to good practice in corrosion control: Bimetallic corrosion. UK Department of Trade and Industry.
  8. Parrott, R., & Pitts, H. (2011). Chloride stress corrosion cracking in austenitic stainless steel: Assessing susceptibility and structural integrity (Research Report RR902). Health and Safety Executive. https://www.hse.gov.uk/research/rrhtm/rr902.htm
  9. Peterson, M. B., & Johnson, R. L. (1953). Friction and wear investigation of molybdenum disulfide I: Effect of moisture (NACA Technical Note 3055). National Advisory Committee for Aeronautics. https://ntrs.nasa.gov/citations/19930083561
  10. Tucker, W. C., Brown, R., & Russell, L. (1990). Corrosion between a graphite/polymer composite and metals. Journal of Composite Materials, 24(1), 92–102. https://doi.org/10.1177/002199839002400105
  11. U.S. Department of Defense [DoD]. (2021). MIL-STD-889D, Galvanic compatibility of electrically conductive materials.
  12. U.S. Nuclear Regulatory Commission [NRC]. (1982). Degradation of threaded fasteners in the reactor coolant pressure boundary of PWR plants (IE Bulletin 82-02). https://www.nrc.gov/reading-rm/doc-collections/gen-comm/bulletins/1982/bl82002.html
  13. U.S. Nuclear Regulatory Commission [NRC]. (2010). Generic aging lessons learned (GALL) report (NUREG-1801, Rev. 2), XI.M18 Bolting integrity. https://www.nrc.gov/reading-rm/doc-collections/nuregs/staff/sr1801/

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.