KALTECKOREA

BlogApplication notes

Why does the broach wear fast and tear the surface?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Regrinding sooner or fitting a new broach is the usual response when the teeth wear fast and the surface tears, but if the conditions that wore the teeth are still there, freshly ground teeth tend to go the same way. What actually lies behind it can be weak EP performance, the wrong viscosity, poor oil delivery to the teeth, clogged gullets, or dull or misground teeth, and sometimes two or more at once.

Background

Pick up a part with a broached keyway or spline bore and the wall is lifted in places like fish scales. Pull the broach and there is work material smeared thinly on the finishing teeth, and the edges have already worn white, not long after the last regrind. Broaching finishes size and surface in a single pull, so there is little chance to rescue a torn surface afterwards, and as the regrind interval shortens, tool cost and line stoppages both rise. A study of slot broaching in aero-engine discs points out that broaching usually comes near the end of the process chain, so a single bad slot can mean losing a part that has already been through a great deal of machining (del Olmo et al., 2022).

A broach carries a row of teeth that rise a little higher one after another, and the height step between two teeth is the thickness that tooth cuts. Each chip sits in the space between teeth, the gullet, and travels with the tooth until it leaves the work. Teeth wear in two places: where the clearance face behind the edge rubs on the freshly cut surface, and where the rake face in front rubs on the curling chip. The main mechanisms are adhesive wear, as work material sticks to the edge and tears away, and abrasive wear from hard particles. The finished surface is the profile printed by the last finishing tooth; the cut per tooth falls from about 80 µm on roughing teeth to a few micrometres on finishing teeth, and cutting speeds are typically 2.5 to 80 metres per minute, far below the 75 to 450 metres per minute of turning or milling (Arrazola et al., 2020).

Once a broach is made, its tooth heights and angles are fixed, and it has been pointed out that the only cutting conditions left to adjust on the floor are, in effect, cutting speed and lubrication (Chingo et al., 2026). Broaching cuts thin chips at low speed, so tool and work stay in sliding contact for a long time, and how well the oil keeps them apart goes a long way to deciding tool life and surface. So when wear and tearing rise together on the same broach, replacing the broach is not enough; what happens between tooth and work has to be looked at too.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the torn parts and the last broach as they are, log which teeth show pickup or wear, the date of the last regrind, and the oil and oil supply in use at the time, and compare them with the cutting oil's technical data sheet, the TDS, and the broach drawing.

Hypothesis 1: weak EP performance

Suspect EP performance first when the material or the oil has changed: after a switch from a chlorinated oil to a chlorine-free one for environmental reasons, after a new material that sticks readily to the edge such as soft, gummy steel or stainless steel, after a general-purpose cutting oil starts doing duty on the broach, or in a tank that has run for years on top-ups alone. Think of the first week after an oil change. Carbon steel keyways come out as before, but the low-carbon steel parts on the same line come off with scaly walls, and the finishing teeth carry a thin silvery film of metal.

The surface a broach tooth has just cut is fresh metal with no oxide film, and the pressure there is too high for an oil film alone to keep the two metals apart. Extreme pressure, or EP, additives carrying sulphur, chlorine or phosphorus react with fresh metal at such pressures and temperatures to form a low-friction protective film, which is why mineral oils with EP additives are described as suited to slow, heavily loaded work such as threading, broaching and tapping (Shokrani et al., 2012). Without enough of that film, work material sticks to the edge as a lump, a built-up edge, and when it breaks away it drags the surface with it and leaves a torn mark. A review of broaching research found adhesion to be a main wear mechanism and reported that sulphur and chlorine compounds in mineral oil limited it (Arrazola et al., 2020). In tapping tests, adding a phosphorus or a sulphur EP agent to a paraffin base oil cut tapping torque considerably, and adding both cut it further; the paper notes that EP agents play an important role in difficult operations such as tapping, broaching and reaming (Nogami & Nakano, 2008).

More EP additive is not the whole answer. In wear tests on steel specimens, the ratio between EP additives of different character mattered more to wear resistance than the amount, and the best combination depended on the chemistry of the steel (Huesmann-Cordes et al., 2014). An oil that served one material well can fall short on another. A fluid's chemistry also changes over its service life, so an oil that suited the job at first can lose performance over time (Brinksmeier et al., 2015).

Start with the edges under a magnifier. Look for work material on the rake faces and edges of the finishing teeth and the few teeth before them, and see whether the teeth with pickup match the side of the bore where the surface is torn. Next, find out what the oil is. Check the EP chemistry and the recommended materials in the TDS and the safety data sheet, the SDS, and send tank oil and new oil from the drum to a laboratory on the same day to compare sulphur, chlorine and phosphorus content. For a direct comparison of EP performance there is a standard test that compares metalworking fluids by tapping torque, and it covers both neat and water-miscible fluids (ASTM International, 2025).

If EP performance looks short, choose the EP chemistry and content again with the supplier, based on the material being cut. If a chlorine-free oil is a must, try sulphur or phosphorus combinations in trial cuts on the same material before deciding. Avoid chlorinated additives on titanium alloys, where they can corrode the machined surface and shorten part life (Shokrani et al., 2012). In a tank that has run on top-ups for a long time, change the oil and see whether pickup and tearing continue on fresh oil.

Hypothesis 2: wrong viscosity

Viscosity drifts when the oil's surroundings change rather than the oil itself: a poorly heated plant in winter, a machine where hydraulic or slideway oil leaks into the tank, a hasty top-up with a different grade, or a change of nozzles or pump. Suppose the first run on a Monday morning, after the plant has cooled over the weekend. The tank oil feels stiffer than usual on the fingers, and the stream from the nozzle sags in a thick rope that does not wet the whole broach. Morning parts show tearing, and it eases in the afternoon once the oil has warmed.

Viscosity works less by lowering friction at the edge directly than by carrying the oil to that spot. The contact between tool and work is rough, so a network of tiny channels forms between them, and how far coolant penetrates those channels changes friction and heat transfer at the contact and so affects surface quality (Wei et al., 2022). A broaching study that compared several water-based fluids measured viscosity, wetting angle and spray droplet size together, and explained the effect of the blend with the lowest cutting load by how well it wetted the edge and penetrated the gaps (Ni et al., 2020). On the other hand, form tapping tests that kept the additive package fixed and changed only viscosity found no effect on torque, while the interaction between base oil and a sulphur additive changed efficiency markedly (Bierla et al., 2008). In short, friction at the edge is set mainly by additive chemistry, and viscosity acts indirectly, through how evenly the oil reaches and penetrates at the teeth.

A viscosity that has moved away from new oil is a signal in itself. If viscosity measured at the same temperature sits above or below new oil, another grade may have mixed in, and whatever has mixed in dilutes the EP additives with it. So the check begins with temperature and viscosity together. Log the tank oil temperature at start-up and in the afternoon, and measure tank oil and new oil at the same temperature by the standard test method for kinematic viscosity, then compare with the TDS value (ASTM International, 2024). Look for streaks of a differently coloured oil in the tank, and for a hydraulic reservoir whose level falls for no clear reason.

If cold oil is the cause, circulate the oil to warm it before production or add temperature control to the tank, and put the first part through only once the oil has settled. If another oil has mixed in, stop the leak first, and if a lot has mixed in, empty the tank and refill with fresh oil. Always top up with the same grade, and when the supply method changes, choose with the supplier a viscosity that spreads well under that method.

Hypothesis 3: poor oil delivery

However good the oil, it is no use if it never reaches the teeth. This is likely after nozzles have been moved for a new fixture or part, when nozzles are half blocked with fines, when a clogged filter cuts the flow, and especially in internal broaching, where the broach disappears into the bore and oil sprayed from outside struggles to reach the teeth inside. Picture the line the day after a fixture change. The nozzle bracket was moved, the oil stream now hits the side of the fixture instead of the broach, and parts come out torn on one wall of the bore only.

A handbook summary of broaching troubles lists improper or insufficient coolant among the causes of galling and pickup (Oberg et al., 2020). When oil cannot collect in front of the teeth, rake face and chip, and clearance face and cut surface, slide against each other dry, and there is no oil present for the EP additives to react from. In broaching studies, adding mineral oil reduced cutting forces, while cutting dry gave poor surface roughness (Arrazola et al., 2020). When oil reaches only part of the broach, the teeth on one side work dry, so tearing and wear gather on that side too.

The first job is to see where the oil lands. With the guard closed, watch one stroke through the window and see whether the stream falls on the teeth just before they enter the work, or strikes the fixture or the broach shank and scatters. Compare flow between nozzles by collecting each for a set time, and check for blocked nozzles and filters. Take the broach out after a stroke and see which teeth are wet with oil; you can then match any section that came out dry against the side of the bore that tore.

Where the stream has been missing the teeth, reset the nozzles against the broach teeth, not the fixture. Aim the stream to wet the rake faces of the teeth just before they enter the work, and for internal broaching add or move nozzles so the whole broach is flooded before the stroke. Put nozzle and filter cleaning on the checklist, and add a nozzle position check to every fixture change.

Hypothesis 4: clogged gullets

Clogged gullets appear when the amount or length of cut grows: when thicker parts start going through the same broach, when speed goes up for output, when the material changes to one with tougher chips, or when the brush or oil jet that clears chips on the return stroke weakens. Take the week a new, longer part number arrives. After each stroke every gullet is packed hard with chips, some of them stuck to the edge as if welded on, and long scratch lines show on the part walls.

Broaching chips are not broken off but curled up and stored in the gullet, so broaches use large rake angles to keep the chip continuous. As cutting speed and the cut per tooth increase, chips grow larger and stiffer, which can make chip removal and tooth breakage a problem. Higher output therefore calls for extra means such as brushing or high-pressure cleaning to clear chips from the gullets before they jam, and when chips interact with the gullet volume, cutting forces can behave differently from what is expected (Arrazola et al., 2020). For the same reason the handbook advises a rounded gullet floor so chips curl easily, and chip breaker grooves to split wide curling chips so they do not clog the gullets; it also lists clogged gullets as a cause of a broach sticking in the work (Oberg et al., 2020). If cutting continues after a gullet is full, the surplus chip is forced between the tooth and the cut surface and scores it, and there is no longer room for oil to collect in front of the tooth.

Look into each gullet of the broach after a stroke. See whether chips fill the gullet to the floor, whether they jammed in flat instead of curling, and whether chips are welded to the edges. Compare the part's length of cut with the design length on the broach drawing, and confirm that the brush and jets that clear chips on the return stroke actually reach the teeth. Also match the position of the scratch lines with the teeth whose gullets were packed.

If chips are clogging the gullets, first make sure every gullet is emptied on every stroke. Realign the brushes and jets to the gullets and replace worn brushes. If parts longer than the broach's design length must be cut, review the gullet size and tooth rise for that part with the broach maker, and for materials with tough chips, look at speed and chip breaker layout together.

Hypothesis 5: dull or misground teeth

The state of the teeth is bound up with regrinding. Consider this hypothesis when the regrind was put off to suit the production plan, when regrinding moved to another shop or another grinder, or when repeated regrinds have left the finishing teeth undersize. On the first day with a broach back from an outside regrind, the edges shine, yet fine streaks are printed on the surface from the first few parts, and a magnifier shows a thin burr left on the edges.

A dull tooth has a rounded edge and a worn band on its clearance face, so it rubs more and cuts less. In slot broaching tests on a heat-resistant alloy, a larger edge radius changed cutting force markedly, with the feed-direction component rising to match the tangential one, and once the edge had worn heavily, strong vibrations appeared in the force signal, surface quality fell and the friction coefficient rose to nearly 1. The same study found grain boundaries beneath the cut surface distorted in the cutting direction (Pérez-Salinas et al., 2023). Regrinding can leave its own marks. A broach is sharpened by grinding the rake face, so the finishing teeth lose a little size with every regrind, and grinding defects can be printed straight onto the broached surface (Arrazola et al., 2020). The handbook likewise lists dull or improperly sharpened broaches among the causes of galling and pickup, and advises grinding accurately so the gullet contour is kept, and taking sharpening burrs off with a wooden block (Oberg et al., 2020).

Judge the teeth by eye and by numbers. Under a magnifier look for the worn band on each clearance face, chipped edges and burrs left by regrinding, and after a regrind compare the rake angle, the gullet contour and the finishing tooth diameter with the broach drawing. If the machine logs load or current, follow how the peak load per stroke climbs after each regrind. Monitoring tool wear during the process by recording force, vibration and motor current together has been studied (del Olmo et al., 2022).

When the wear band and load trend point to dull teeth, set the regrind point by a limit on wear band width or peak load rather than by the calendar. When regrinding is outsourced, write rake angle, gullet contour and burr removal into the acceptance criteria, and measure and inspect each broach before use. Once the finishing teeth have reached the lower size limit on the drawing, stop stretching it with regrinds; it is time for a new broach.

Finding the cause

There is no need to dig through all five at once. Clear away first what can be seen without a long stop. Where the oil lands and whether the gullets are empty after a stroke show up within a stroke or two. Oil temperature and top-up records can be checked straight away. Viscosity and composition analysis and measuring the teeth need samples sent out or the broach pulled, so they come next.

The shape of the tearing also points the way. If it gathers on one wall or one section, look at whether oil reaches those teeth or chips clog those gullets. If metal sticks to the edges, the whole circumference tears evenly, and it began right after a change of material or oil, look towards EP performance and viscosity. Damage that worsens steadily in the days after a regrind points to dull teeth; streaks from the very first parts after a regrind point to the grinding itself. If it changes with the time of day, bad in the morning and better in the afternoon, check oil temperature and viscosity first.

If that still does not settle it, run control trials that change one thing at a time. Brush new oil from the drum directly onto the broach in place of tank oil and cut a few parts, add one more nozzle, empty the gullets by hand before cutting, or switch to a freshly reground and inspected broach. Change only one thing at a time, or there is no telling which one worked. Judge by counting torn parts and peak load per stroke on the same material lot, on the same basis as before the change.

The final check is to run a full regrind interval in the corrected state. Good first parts are not enough: follow pickup on the edges, wear band width and the number of torn parts through to the next regrind, and the job is done only when the number of parts between regrinds has grown.

The hypotheses often interlock. Dull teeth rub more and raise heat and adhesion, so even the same oil can look short on EP performance, and a gullet packed with chips leaves no room for oil, so the tooth works dry even when delivery is right. In such cases fix what can be put right by eye first, chip clearing and oil delivery, take a freshly ground and inspected broach as the baseline, and only then judge the oil's EP performance and viscosity. While the teeth and chips are unsettled, the effect of changing the oil cannot be compared fairly.

Limits and cautions

Suitable cutting speed, tooth rise, the oil's EP chemistry and viscosity, and regrind criteria differ by material, broach design and machine, so numeric decisions follow the cutting oil's TDS and the broach maker's guidance. For parts such as aircraft components, where damage below the surface must be controlled as well, do not accept parts on floor judgement alone; go through laboratory checks such as cross-section structure and residual stress, and confirmation by the quality engineer. Chlorinated additives carry environmental rules and waste oil conditions, so check company standards and the disposal contractor's terms before changing oil.

Safety matters too. Follow the product's SDS for protective equipment and ventilation when handling cutting oil. Metalworking fluids can harm health through skin contact and through breathing in mist (OSHA, n.d.). Pull the broach, clear gullets or inspect teeth only after the machine is fully stopped and locked out, and since broach teeth are sharp and the tool is heavy, wear gloves and handle it on a rest.

Sources

  1. Arrazola, P. J., Rech, J., M'Saoubi, R., & Axinte, D. (2020). Broaching: Cutting tools and machine tools for manufacturing high quality features in components. CIRP Annals, 69(2), 554–577. https://doi.org/10.1016/j.cirp.2020.05.010
  2. ASTM International. (2024). ASTM D445-24, Standard test method for kinematic viscosity of transparent and opaque liquids (and calculation of dynamic viscosity). https://store.astm.org/d0445-24.html
  3. ASTM International. (2025). ASTM D8288-25, Standard test method for comparison of metalworking fluids using a tapping torque test machine. https://store.astm.org/d8288-25.html
  4. Bierla, A., Fromentin, G., Martin, J. M., Le Mogne, T., Minfray, C., & Genet, N. (2008). Evaluation of lubricant viscosity and base oil effects by form tapping test [Conference paper]. HAL. https://hal.science/hal-00910301
  5. Brinksmeier, E., Meyer, D., Huesmann-Cordes, A. G., & Herrmann, C. (2015). Metalworking fluids—Mechanisms and performance. CIRP Annals, 64(2), 605–628. https://doi.org/10.1016/j.cirp.2015.05.003
  6. Chingo, C. M., Ortiz-de-Zarate, G., Rodriguez, I., Etxebeste, M., & Arrazola, P. J. (2026). Effects of cutting speed and lubrication on surface topography in broaching of 42CrMo4 steel. Procedia CIRP, 144, 555–560. https://doi.org/10.1016/j.procir.2026.02.033
  7. del Olmo, A., López de Lacalle, L. N., Martínez de Pissón, G., Pérez-Salinas, C., Ealo, J. A., Sastoque, L., & Fernandes, M. H. (2022). Tool wear monitoring of high-speed broaching process with carbide tools to reduce production errors. Mechanical Systems and Signal Processing, 172, 109003. https://doi.org/10.1016/j.ymssp.2022.109003
  8. Huesmann-Cordes, A. G., Meyer, D., Brinksmeier, E., & Schulz, J. (2014). Influence of additives in metalworking fluids on the wear resistance of steels. Procedia CIRP, 13, 108–113. https://doi.org/10.1016/j.procir.2014.04.019
  9. Ni, J., Feng, K., He, L., Liu, X., & Meng, Z. (2020). Assessment of water-based cutting fluids with green additives in broaching. Friction, 8(6), 1051–1062. https://doi.org/10.1007/s40544-019-0318-y
  10. Nogami, T., & Nakano, K. (2008). Interaction between additives in metalworking fluids under difficult cutting conditions. Tribology Online, 3(3), 177–180. https://doi.org/10.2474/trol.3.177
  11. Oberg, E., Jones, F. D., Horton, H. L., & Ryffel, H. H. (2020). Machinery's handbook (31st ed.). Industrial Press.
  12. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids
  13. Pérez-Salinas, C., Fernández-Lucio, P., del Olmo, A., Aldekoa-Gallarza, I., & López de Lacalle, L. N. (2023). The influence of cutting edge microgeometry on the broaching of Inconel 718 slots. Engineering Science and Technology, an International Journal, 48, 101563. https://doi.org/10.1016/j.jestch.2023.101563
  14. Shokrani, A., Dhokia, V., & Newman, S. T. (2012). Environmentally conscious machining of difficult-to-machine materials with regard to cutting fluids. International Journal of Machine Tools and Manufacture, 57, 83–101. https://doi.org/10.1016/j.ijmachtools.2012.02.002
  15. Wei, W., Robles-Linares, J. A., Liao, Z., Wang, Z., Garcia Luna, G., Billingham, J., & Axinte, D. (2022). On modelling coolant penetration into the microchannels at the tool-workpiece interface. Journal of Manufacturing Processes, 84, 43–54. https://doi.org/10.1016/j.jmapro.2022.09.044

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.