BlogApplication notes
Why does conveyor chain stretch so quickly?
- Type
- Application notes
- Published
- 23 November 2026
- Prepared by
- Jonghwan Moon
- Product group
- Equipment/Service Lubricants
Taking out links or replacing the whole chain is the usual response to conveyor chain stretch, but chain usually lengthens because the pins and bushes inside its joints wear, not because the plates stretch, so unless the conditions that sped up that wear are fixed, a new chain will soon stretch fast again. What actually lies behind it can be oil not reaching the pins and bushes, abrasion by dust and wear debris, the wrong viscosity, infrequent lubrication or corrosion after washdown, and sometimes two or more at once.
Background
The take-up bolts are at the end of their travel, yet the conveyor chain still sags and surges, and as it goes round the sprocket the rollers ride up towards the tooth tips and clunk. Two links were taken out a few months ago to make up for the stretch, and the chain is already back where it was. In the maintenance log, the chain replacement dates keep getting closer together.
A stretched chain no longer meshes properly with its sprockets, so it jumps teeth or wears the sprocket teeth as well, and the spacing between attachments changes, so products land in the wrong place. Replacing chain and sprockets together means stopping the line, and the shock when the chain jumps a tooth can spread damage to other parts. The more often replacement comes round, the more the stopped line outweighs the cost of the parts.
Chain does not usually lengthen because its link plates stretch. The pin and bush in each joint wear, the clearance between them grows, and the small clearances of hundreds of joints add up to a longer chain (Sappok & Sauer, 2015). Each time the chain wraps onto and leaves a sprocket, every joint flexes a little and the pin and bush slide under load, so the joint works in boundary lubrication with almost no oil film and is sensitive to oil condition and contamination (Paulovics et al., 2022). Chain life is set by this elongation, and chain is said to start jumping sprocket teeth at around 3% elongation (Noguchi et al., 2009).
In such cases the technical team sets up the five hypotheses below and rules them out one by one. Whichever hypothesis it turns out to be, the first job is the same: measure the length of a set section of chain to put a number on the percentage stretch against new chain and on how fast it is rising, and compare the lubricant's technical data sheet, the TDS, the method of lubrication and the interval with the chain maker's instructions.
Hypothesis 1: oil not reaching pins
If a chain always looks wet with oil yet stretches quickly, start with this hypothesis. It covers lubricators that drip onto the rollers or the middle of the chain, brushes that only coat the outside, and chains run on the factory lubrication alone with no further oiling. The conveyor chain on one packing line always looks glossy. The lubricator nozzle is aimed at the rollers in the middle of the chain, so the rollers and the floor beneath have plenty of oil, yet when the chain is flexed by hand some joints catch stiffly.
Chain wear happens not on the outside but inside the joint, in the narrow gap where pin meets bush. The only way for oil to reach that gap is through the clearances between the inner and outer link plates, so oil has to be applied to the upper edges of the link plates on the slack span to work into the joint, and oil applied only to the rollers does not get enough into the joint (Diamond Chain Company, n.d.). In a joint the oil has not reached, pin and bush slide dry. In one experiment that reproduced wear with just two links, the pin bent slightly under tension, so pin and bush wore only at the ends of the pin, not the middle (Noguchi et al., 2009). The oil, then, has to reach the ends of the joint, close to the link plates.
Stop the chain and flex a few joints by hand. See whether they bend smoothly or some catch, whether oil is seeping from the gaps between the link plates, and whether the area around the pins is dry. A stiff joint can come from foreign matter, poor lubrication or corrosion inside the joint, so weigh it alongside the other hypotheses (Diamond Chain Company, n.d.). Check where the lubricator nozzle or brush is aimed and whether it sits on the slack span, and if a length of chain has been removed, press out a pin and look at the wear marks and any traces of oil at its ends.
Correct the point of application first. Move the nozzle or brush to the upper edges of the link plates on the slack span, where inner and outer plates overlap, and set it to reach both rows of plates. A chain that has run dry for a long time should be cleaned and soaked well in oil so the joints fill before it goes back on. From then on, include a check that oil is seeping into the plate gaps right after lubrication.
Hypothesis 2: abrasive dust
In processes where powder flies, such as cement, feed, timber or foundry sand, dust is the next suspect. Chains running close to the floor, sections where material spills onto the chain, and chains that are often recoated with sticky oil deserve a look too. Wipe the chain on a feed mill transfer conveyor and the rag comes away with brownish-grey paste rather than oil. The paste fills every joint gap, and the lubricator keeps adding oil on top.
Oil holds on to dust. The hard particles it catches travel with the oil between pin and bush and cut both surfaces; in tests of wear by particles trapped between two surfaces, more angular particles caused more wear (Stachowiak & Stachowiak, 2001). The way particles in a lubricant are drawn into a contact and cut the surfaces has been studied far enough in bearings to build models that predict the wear (Dwyer-Joyce, 1999). Engine timing chain research has also developed a friction test on real pins and bushes that compares clean oil with oil blended with carbon black, and wear rose once the contaminant passed a certain amount (Paulovics et al., 2021, 2022).
The debris from the joints is the first evidence. Rub it between the fingers to feel for grit, and dissolve it in solvent and filter it to see the amount and shape of the particles left. A laboratory can look at elements from dust, such as silicon, alongside wear elements such as iron. Find where powder falls onto the chain and where the chain drags through floor debris, and if the same chain runs somewhere less dusty, compare how fast each one stretches.
Reducing the ways powder reaches the chain comes first. Fit guards and covers, stop material spilling onto the chain, and clear debris from under it regularly. Chain should be protected from abrasive and corrosive conditions and its oil supply kept free of contamination, and a chain packed with debris is cleaned with an approved solvent and then relubricated (Diamond Chain Company, n.d.). Giving the right amount of an oil that penetrates the joints can hold less dust than piling on sticky oil.
Hypothesis 3: wrong viscosity
Viscosity problems arise when one oil covers every chain in a plant, when heavy gear oil or grease is put on chain, or at the other extreme when only a thin rust preventive or spray lubricant goes on. Using the same oil on chains in places as different as a cold store and a drying oven does the same. The conveyor chain at the cold store entrance always carries a thick coat of grease. The outside of the link plates is covered, yet flex a joint and the inside is dry, with dry powder coming from around the pin.
Two demands pull on oil viscosity. To get into the joint it must be thin enough to flow through the gaps between the link plates, and once inside it must be thick enough to form a film that keeps pin and bush apart. The oil with the highest viscosity that will still flow between the plates and fill the pin-bush area therefore gives the best wear life, while heavy oils and greases are generally too stiff to enter the joints (Diamond Chain Company, n.d.). Too thin is a problem as well: low-viscosity engine oils have been reported to worsen timing chain wear (Sappok & Sauer, 2015). In friction tests on pins and bushes, too, the highest of the three viscosity grades compared gave the least wear (Paulovics et al., 2022).
Put the TDS and the actual temperature side by side. Check the kinematic viscosity at 40 °C and the working temperature range in the TDS of the oil or grease in use, and measure the actual temperature where the chain runs. Viscosity changes strongly with temperature, so the same oil can be too thick in a cold store and too thin near a drying oven. See whether oil seeps into the plate gaps right after application, flex a joint a few hours later to see whether it is still wet inside, and check whether a thick outer layer of lubricant has become a dust trap.
The fix lies in the choice of oil. Reselect the viscosity to suit the ambient temperature where the chain runs, using the chain maker's table of recommended viscosity by surrounding temperature as the basis (Diamond Chain Company, n.d.). Do not manage chains in cold and hot places on one oil, and for chains that have been greased, scrape off the outer grease and change to an oil that penetrates the joints. Where ordinary oil evaporates quickly, as in high-temperature sections, agree a dedicated chain lubricant for that temperature with the supplier.
Hypothesis 4: infrequent lubrication
Lubrication becomes infrequent for many reasons: an automatic lubricator stops or runs with an empty tank unnoticed, manual oiling drops out of the shift routine, or output goes up and running hours lengthen while the interval stays the same. Take a line that used to run days only and now runs into the night, still oiled once on Monday morning. By the end of the week the chain sounds dry going round the sprockets, and it is quiet only on the day it was oiled.
Lubrication is not a one-off. Oil in the joints is gradually pushed out and scattered in service, and chain lubrication does more than resist wear: it cushions shock, carries away heat, flushes out foreign matter and prevents rust (Diamond Chain Company, n.d.). A joint short of oil relies on a thin boundary film and eventually passes into direct metal contact, with friction and wear rising accordingly (Stachowiak & Batchelor, 2014). If running hours lengthen but an interval set by the calendar stays the same, the time the joints run dry between oilings grows.
One calculation shows it. Match the lubrication records with the running-hour records to find how many hours the chain runs between oilings, and compare that with the chain maker's recommended interval. For an automatic lubricator, check the tank level, the pump and the nozzles for blockage, and compare the joints by flexing or by sound just before and just after oiling. If elongation has been measured at regular intervals, see whether it sped up in periods when oiling was missed.
Set the interval by running hours, not by the calendar. Base the new interval on the chain maker's inspection intervals and recommended method, and revise it whenever operating conditions change. Give automatic lubricators a low-level alarm and a routine check, and for manual oiling add a sign-off box for each shift. Relubricating a chain that went without for long does not shrink clearances that have already grown, so measure the elongation to judge the life remaining.
Hypothesis 5: washdown corrosion
Where lines are washed often with water and detergent, as in food, beverage and meat processing, washdown may be driving the wear. This is especially so when high-pressure water hits the chain directly, when acid or chlorinated cleaners are used, and when there is no relubrication step after washing. A meat processing line is hosed down at high pressure at the end of every shift. By morning reddish rust water has spread between the link plates, and the work instructions have no step for oiling again after washing.
Washwater strips the oil from the joints and leaves water and cleaner in its place. The joints then run dry and rust at the same time, and when wear and corrosion act together the loss can exceed the sum of each measured alone, a synergy for which measurement methods have been developed (Watson et al., 1995). Stainless chain is not safe either. Stainless steel resists corrosion through a thin passive film on its surface, and when rubbing contact strips that film, the exposed metal corrodes and the film re-forms, over and over, with material lost each time (Landolt & Mischler, 2011). Rust inside the joints makes them stiff, and chain that has seized this way ends up being replaced (Diamond Chain Company, n.d.).
Look at the chain on the morning after a washdown. Check for rust water or red powder in the joint gaps and around the pins, and flex a few joints for stiffness. Compare the work instructions with what is actually done: cleaner type and strength, washing pressure, whether the chain is sprayed directly, and whether there is a drying and relubrication step afterwards. Confirm from the chain maker's literature that the chain material suits that cleaner.
Make washing and lubrication one package. Change the washing method so high-pressure water is not aimed straight at the chain, and add a step to the instructions to dry off the water and relubricate straight after washing. Resistance to washing off is compared from product data, and for greases there is a standard test of how well the grease stays on a metal surface under a water spray (ASTM International, 2020). On food lines, choose, among food-grade products, one that has water resistance data. Replace chain whose joints have seized with rust, and if corrosion continues, consider chain in a material suited to the cleaner.
Finding the cause
Putting a number on the stretch is the starting point. Roller chain length accuracy is specified as the length of a set section under a set measuring load (ISO, 2015), so on the floor too, measure the same section the same way with the chain under light tension, or the readings cannot be compared. One chain maker's guidance has chain replaced once it has stretched beyond 3%, with 1.5% as the limit on fixed-centre drives (Diamond Chain Company, n.d.). The rate of stretch says more about the cause than any single reading.
Next come the things that can be checked without a long stop. The point of application and interval, the lubricator's operation, the washdown routine and dust around the chain can be confirmed at once by eye and from the records, so rule them out at this stage. Judge viscosity and contaminant particles from the TDS and from samples, and look at pins and bushes when a length of chain comes off.
The look of the chain points to the cause. A chain wet outside but dry and stiff in the joints suggests the point of application or viscosity; grey paste packed in the joint gaps suggests dust; rust water and red powder prominent the morning after washdown suggest washdown. If the stretch sped up while oiling was being skipped, look at the interval, and if only chains in extreme temperatures such as cold stores or drying ovens stretch unusually fast, look at viscosity.
A comparison trial is easy where a conveyor has two strands running side by side or where identical lines exist. Change the point of application or the oil on one side only, measure the same section at the same running hours, and compare the rates of stretch. Change one thing at a time, and keep the rate of stretch before the change as the baseline.
The hypotheses overlap. A joint washed free of oil rusts dry if oiling comes late, and a chain coated in sticky grease keeps oil out of its joints while trapping dust. In such cases, set the point of application, viscosity and interval right first so the joints are full of oil, then look at dust and washdown again. While the joints are empty, there is no gauging how much dust or rust is adding.
Limits and cautions
The right lubricant, viscosity, lubrication interval and replacement limit differ with chain type and size, speed, load and surroundings, so numeric decisions follow the chain maker's instructions and the lubricant TDS. Conveyor chains have a standard of their own, separate from transmission roller chains (ISO, 2006), and chains with attachments or special rollers may follow different maker criteria. Do not join a section of new chain to a stretched one, and when replacing chain, check the sprocket teeth for wear as well.
Where chain meets sprocket, hands are easily caught. Measure length, check joints, adjust lubricator nozzles and wash only with the equipment stopped and locked out, following the rules for controlling hazardous energy (OSHA, n.d.). An inclined conveyor or a chain carrying a load can move under its own weight even with the power off, so secure it before work. Handle cleaners, solvents and lubricants with the protective equipment and ventilation set out in the safety data sheet, the SDS.
Sources
- ASTM International. (2020). ASTM D4049-20, Standard test method for determining the resistance of lubricating grease to water spray. https://store.astm.org/d4049-20.html
- Diamond Chain Company. (n.d.). Diamond Chain maintenance guide. Retrieved November 2026. https://www.timken.com/resources/diamond-chain-maintenance-guide/
- Dwyer-Joyce, R. S. (1999). Predicting the abrasive wear of ball bearings by lubricant debris. Wear, 233–235, 692–701. https://doi.org/10.1016/S0043-1648(99)00184-2
- International Organization for Standardization [ISO]. (2006). ISO 1977:2006, Conveyor chains, attachments and sprockets.
- International Organization for Standardization [ISO]. (2015). ISO 606:2015, Short-pitch transmission precision roller and bush chains, attachments and associated chain sprockets.
- Landolt, D., & Mischler, S. (Eds.). (2011). Tribocorrosion of passive metals and coatings. Woodhead Publishing. https://doi.org/10.1533/9780857093738
- Noguchi, S., Yoshiba, H., Nakayama, S., & Kanada, T. (2009). Evaluation of wear between pin and bush in roller chain. Journal of Advanced Mechanical Design, Systems, and Manufacturing, 3(4), 355–365. https://doi.org/10.1299/jamdsm.3.355
- Occupational Safety and Health Administration [OSHA]. (n.d.). Control of hazardous energy (lockout/tagout). U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/control-hazardous-energy
- Paulovics, L., Kuti, R., Rohde-Brandenburger, J., & Tóth-Nagy, C. (2021). Development of comparative investigation method for timing chain wear analysis using oscillating tribometer. Acta Technica Jaurinensis, 14(4), 406–423. https://doi.org/10.14513/actatechjaur.00620
- Paulovics, L., Rohde-Brandenburger, J., & Tóth-Nagy, C. (2022). Timing chain wear investigation methods: Review. FME Transactions, 50(3), 461–472. https://doi.org/10.5937/fme2203461P
- Sappok, D., & Sauer, B. (2015). Wear measurement on chain joint components using a roundness instrument. Periodica Polytechnica Mechanical Engineering, 59(2), 51–59. https://doi.org/10.3311/PPme.7780
- Stachowiak, G. B., & Stachowiak, G. W. (2001). The effects of particle characteristics on three-body abrasive wear. Wear, 249(3–4), 201–207. https://doi.org/10.1016/S0043-1648(01)00557-9
- Stachowiak, G. W., & Batchelor, A. W. (2014). Engineering tribology (4th ed.). Butterworth-Heinemann.
- Watson, S. W., Friedersdorf, F. J., Madsen, B. W., & Cramer, S. D. (1995). Methods of measuring wear-corrosion synergism. Wear, 181–183, 476–484. https://doi.org/10.1016/0043-1648(95)90161-2