KALTECKOREA

BlogApplication notes

Why do copper and brass parts tarnish after cleaning?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Cleaning & Surface Prep

Reworking tarnished copper or brass parts by pickling or polishing is the usual response, but if the cleaning conditions that caused the tarnish stay the same, the next lot comes out the same colour. What actually lies behind it can be complexing agents such as chelants or ammonia that dissolve copper, a cleaner with no azole inhibitor, copper ions built up in the bath, high temperature and long time, or slow drying, and sometimes two or more at once.

Background

Brass fittings and copper terminals that went into the washer to remove oil come out with pinkish blotches instead of a yellow sheen, or darken to brown and black within a day or two of storage. Parts rejected at visual inspection must be pickled again or polished back to a shine, which costs more processing and labour and can push back deliveries. It may not end at appearance. A surface oxide film can get in the way of later plating, soldering or electrical contact, which is why copper alloys are taken through a tarnish removal step before plating (ASTM International, 2025).

Copper changes colour as copper oxides form on its surface in contact with air and water. The first corrosion product on copper in the atmosphere is cuprous oxide, cuprite, which looks black when the layer is thin, and the colour depends on the amount and composition of the products (FitzGerald et al., 2006). Brass, an alloy of copper and zinc, also changes colour another way. When zinc leaves, the surface turns from yellow to the salmon pink of pure copper, and if that copper then corrodes to cuprite it goes reddish and then brown (Selwyn, 2019).

Cleaning removes not only oil but also the thin oxide and protective films that covered the surface, so freshly cleaned copper is more reactive than before. Tarnish therefore appears when the cleaning solution dissolves copper directly, when nothing is there to protect it, when conditions are too severe, or when water stays on the part too long after washing.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: set aside tarnished parts alongside sound ones, check the cleaner's composition in its technical data sheet, the TDS, and safety data sheet, the SDS, and then compare concentration, temperature, immersion time, the date of the last bath change, and the rinsing and drying methods against the records.

Hypothesis 1: complexing agents

Look at this hypothesis first when the cleaner contains chelating agents that bind strongly to metal ions, such as EDTA, citrate or gluconate, added to handle hardness or rust, or when it contains amines or ammonia. It applies especially on lines where a general-purpose cleaner chosen for steel parts is also used on copper alloy parts. Take a line that washes steel brackets and brass fittings in one basket with the same alkaline cleaner. The steel comes out clean, but the brass fittings lose their shine and show pinkish blotches here and there.

A chelating agent, like any complexing agent that binds metal ions into complexes, wraps metal ions and holds them in solution, opening a route for the surface oxide film to dissolve. In experiments dissolving copper oxide in EDTA solutions, the oxide did not dissolve without EDTA and did dissolve with it (Tamura et al., 2001). Once the oxide film is gone, the copper beneath is exposed, and that copper oxidises again to an uneven colour. Ammonia also forms complexes with copper, and the rate at which copper dissolves in aqueous ammonia was studied early on (Halpern, 1953). For brass, acidic solutions, alkaline solutions and polishes containing ammonia can all cause dezincification, the loss of zinc, and its first sign is a colour change towards pink (Selwyn, 2019).

The ingredient list is the first clue. Check the SDS and TDS for chelating agents, amines or ammonia, and whether the cleaner is stated as suitable for copper alloys. Then make up the same cleaner fresh in a beaker at working concentration and temperature, immerse freshly cleaned copper and brass coupons, and compare their colour with coupons in a cleaner without chelating agents. A deepening pink points to zinc loss; an overall dull darkening points to the oxide film dissolving and re-forming.

If the cause narrows to complexing agents, switch to a cleaner made for copper alloys, or gather copper alloy parts and wash them in a separate tank. If chelating agents were needed because of hard water, making up the bath with softened or deionised water can be an alternative. After changing cleaners, confirm that oil still comes off well enough.

Hypothesis 2: no azole inhibitor

Protection for copper may be missing where the cleaner was chosen for steel and aluminium parts, right after a switch to a cheaper cleaner, after the supplier changed the formulation, or where the cleaner is heavily diluted with water. Consider a month in which the cleaner was swapped for another product to cut costs. Straight after washing nothing looked different, but bundles of copper terminals left in the store for a day are evenly darkened the next morning.

Azole inhibitors such as benzotriazole or tolyltriazole are used to protect copper from corrosion, and a review of copper corrosion inhibitors treats azole compounds as the leading inhibitors for protecting copper (Antonijević & Petrović, 2008). A review devoted to benzotriazole shows that it adsorbs onto the copper surface and forms a thin polymeric complex film bound to cuprous ions, blocking the reactions by which oxygen and water reach the copper, and that the effect varies with conditions such as pH, temperature and inhibitor concentration (Finšgar & Milošev, 2010). Copper washed in a cleaner without inhibitor goes through rinsing, drying and storage with its oxide film stripped, fully exposed to air and moisture all the while.

Check the TDS for wording that the cleaner suits copper alloys or brass, so-called yellow metals, and that it contains a corrosion inhibitor. If in doubt, ask the supplier whether an azole inhibitor is present and whether the inhibitor level in the working bath can be analysed. On the floor, put identical copper coupons in fresh and in used solution for the same time, dry them the same way, and compare their colour a day later.

If the inhibitor appears to be missing, switch to an inhibited cleaner suitable for copper alloys. Even in a product that contains an inhibitor, the level can fall in use, so manage it by the supplier's method, and review with the supplier whether to add an inhibitor step at the final rinse or before storage.

Hypothesis 3: copper build-up

Copper builds up in the bath where the solution goes a long time between changes, where many copper and brass parts are washed, or where a chelating cleaner slowly dissolves copper. When the solution starts to take on a faint blue tint, it is time to suspect this hypothesis. Suppose a pattern repeats: no trouble in the week after a bath change, then tarnish rejects climb from the point, some weeks on, when the solution turns bluish, and a fresh change brings a quiet spell again.

Dissolved copper ions can themselves act as an oxidant for copper. In solutions of cupric ions bound to ammonia, copper metal dissolved, and faster at higher temperature and rotation speed (Uchida et al., 1996). In a study in sulphuric acid solution as well, adding cupric ions together with oxygen increased the amount of copper metal dissolved (Yoo et al., 2020). On brass, copper and zinc have been observed to dissolve together, with copper then redepositing on the surface (Zhou et al., 2017), and redeposited copper can show as uneven reddish blotches. Since azole inhibitors build their film by binding copper ions, a high level of copper ions in the bath may also use up the inhibitor before it reaches the surface.

Look at the bath's copper level as a number. Draw samples at regular intervals and have the supplier or a laboratory analyse them for copper, or get a rough value with copper test strips on the floor. Overlay those values on the days since the last change and the tarnish reject rate to see whether they rise together. Comparing the colour of identical coupons in fresh and in long-used solution is another quick check.

If copper ions are the cause, tie bath changes to copper concentration rather than to the calendar. Dissolved copper is not caught by particle filters, so it has to be brought down by changing or partly replacing the solution. If many copper alloy parts are washed, give them a tank of their own, and set with the supplier an upper limit for the copper level the solution can tolerate.

Hypothesis 4: heat and long soaks

Tarnish can increase when the bath temperature was raised because oil was not coming off, when ultrasonic cleaning time was extended, when a basket stays submerged while the line is stopped, or when parts are held as the anode for a long time in electrolytic cleaning. One such case: the conveyor stopped over lunch and a basket sat in the hot tank for nearly an hour, and only the brass parts from that basket came out noticeably dark and blotchy.

Temperature and time amplify every reaction the earlier hypotheses describe. The rate at which copper dissolved in cupric ion solutions rose with temperature and with stronger flow (Uchida et al., 1996). The longer the soak, the more dissolves and oxidises. The standard for preparing copper alloys for plating also cautions that prolonged anodic cleaning can cause slight tarnishing or etching, particularly of brass (ASTM International, 2025). Since the protective film an inhibitor builds also varies in effect with temperature (Finšgar & Milošev, 2010), a cleaner that caused no trouble at room temperature may fail to protect copper at high temperature.

Start by seeing whether tarnish clusters in certain baskets or certain times of day. Match bath temperature records and line stoppage records against the tarnished lots, and measure how long baskets actually stay in the tank. Immersing coupons at the low and high ends of the TDS temperature range, and for short and long times, shows at which conditions the colour starts to change.

If temperature and time are the cause, reset to the lowest temperature and shortest time that still remove the oil. Change the equipment or work rules so baskets are lifted out when the line stops, and for electrolytic cleaning set time and current to the TDS and the supplier's guidance. If the temperature was raised because oil was not coming off, look for that cause separately, in cleaner concentration or in the type of oil from the upstream process.

Hypothesis 5: slow drying

This hypothesis gains weight when rinsed parts air-dry in their baskets, when parts have recesses or holes that hold water, when wet parts are stacked, in the humid rainy season, or when rinse water goes long unchanged and carries cleaner. Parts washed late in the afternoon are left in their baskets to dry overnight, and the next morning brown and black rings remain along the paths where water ran off and in the recesses where it pooled.

Metals corrode in air because reactions take place in a thin water film on the surface, and the longer the surface stays wet, the further corrosion proceeds (Leygraf et al., 2016). When freshly cleaned copper, its oxide film thinned, sits under a drop of water for a long time, cuprite grows there first, and since a thin cuprite layer looks black (FitzGerald et al., 2006), a stain is left in the shape of the drop. If cleaner remains in the rinse water, its components concentrate in small spots as the water evaporates, and those spots tarnish faster.

The shape and position of the stains tell the story. If they cluster along run-off paths, in recesses where water pooled, where parts touched the basket, or on faces stacked against each other, drying is a likely cause. Record how long parts take to dry after rinsing and the temperature and humidity of the drying area, and measure the conductivity of the rinse water to see how much cleaner it carries.

If drying is the cause, remove the water fast and completely. Do the final rinse in clean or deionised water, dry with hot air straight after rinsing, set part orientation so water drains, and never stack wet parts. Pack fully dried parts in moisture-resistant packaging and store them somewhere dry, and if needed review a protective treatment before storage with the supplier.

Finding the cause

Of the five hypotheses, clear first those that documents and records can settle. Cleaner composition is in the SDS and TDS, and temperature, time and bath change dates are in the work records, so complexing agents, inhibitors, and temperature and time can largely be settled without immersing a single coupon. The bath's copper level needs a laboratory analysis, so look at drying and stain shapes while waiting.

Colour and pattern give the direction. Pink on brass means zinc has left or copper has redeposited, so look at chelating agents, ammonia, accumulated copper ions and severe temperature and time; an even darkening of copper and brass points to a missing inhibitor or to copper built up in the bath. Stains shaped like drops and run-off point to drying, tarnish concentrated in particular baskets or times of day points to temperature and time, and tarnish that grows day by day after a bath change points to accumulated copper ions.

If that still does not settle it, run a control test with coupons. Immerse identical copper and brass coupons in fresh and in used solution, in the current cleaner and in one made for copper alloys, and at low and high temperature, then split them again on removal between hot-air drying straight away and air-drying. Change only one condition at a time, or there is no telling what changed the colour. Compare colours under the same lighting, and grading the tarnish with photographs, much as the copper strip corrosion test for petroleum products grades it against colour standards, makes comparison easier (ASTM International, 2019).

Confirm the outcome on real parts. Wash several lots under the changed conditions, check their colour straight after washing and after a set storage period, and see whether the tarnish reject rate, counted on the same basis as before, has fallen. Some tarnish appears only later in storage, so do not stop at checking straight after washing.

The hypotheses can overlap. A chelating cleaner dissolves copper and builds copper ions in the bath, accumulated copper ions and high temperature drive each other's reactions, without an inhibitor all of this lands on the surface, and slow drying then sets it as stains. In such cases, correct cleaner composition, temperature and time first, change the bath, and only then look at drying, because while the bath side is unsettled the effect of changing the drying cannot be compared fairly.

Limits and cautions

Cleaner concentration, temperature, time, inhibitor level and bath change rules differ by product and part, so numeric decisions follow the cleaner's TDS and the supplier's guidance. For parts whose surface condition affects function, such as for plating, soldering or electrical contact, do not judge by colour alone; confirm with the tests for that process and the customer's criteria. Pickling and polishing to remove tarnish can take off material, so keep them within dimensional and surface specifications.

Safety matters too. For cleaners and pickling solutions, follow the product's SDS for protective equipment and ventilation, and avoid breathing vapour from products containing ammonia or amines. Do not pour solution or rinse water carrying dissolved copper straight into ordinary drains; dispose of it according to the applicable regulations. Take care against burns when lifting baskets out of hot tanks.

Sources

  1. Antonijević, M. M., & Petrović, M. B. (2008). Copper corrosion inhibitors. A review. International Journal of Electrochemical Science, 3(1), 1–28. https://doi.org/10.1016/S1452-3981(23)15441-1
  2. ASTM International. (2019). ASTM D130-19, Standard test method for corrosiveness to copper from petroleum products by copper strip test. https://store.astm.org/d0130-19.html
  3. ASTM International. (2025). ASTM B281-88(2025), Standard practice for preparation of copper and copper-base alloys for electroplating and conversion coatings. https://store.astm.org/b0281-88r25.html
  4. Finšgar, M., & Milošev, I. (2010). Inhibition of copper corrosion by 1,2,3-benzotriazole: A review. Corrosion Science, 52(9), 2737–2749. https://doi.org/10.1016/j.corsci.2010.05.002
  5. FitzGerald, K. P., Nairn, J., Skennerton, G., & Atrens, A. (2006). Atmospheric corrosion of copper and the colour, structure and composition of natural patinas on copper. Corrosion Science, 48(9), 2480–2509. https://doi.org/10.1016/j.corsci.2005.09.011
  6. Halpern, J. (1953). Kinetics of the dissolution of copper in aqueous ammonia. Journal of The Electrochemical Society, 100(10), 421–428. https://doi.org/10.1149/1.2780873
  7. Leygraf, C., Odnevall Wallinder, I., Tidblad, J., & Graedel, T. (2016). Atmospheric corrosion (2nd ed.). Wiley.
  8. Selwyn, L. (2019). Preventing and treating the dezincification of brass (CCI Notes 9/13). Canadian Conservation Institute. https://www.canada.ca/en/conservation-institute/services/conservation-preservation-publications/canadian-conservation-institute-notes/dezincification-brass.html
  9. Tamura, H., Ito, N., Kitano, M., & Takasaki, S. (2001). A kinetic model of the dissolution of copper(II) oxide in EDTA solutions considering the coupling of metal and oxide ion transfer. Corrosion Science, 43(9), 1675–1691. https://doi.org/10.1016/S0010-938X(00)00171-2
  10. Uchida, S., Takemura, I., Tokuda, M., & Osseo-Asare, K. (1996). The kinetics of dissolution of copper and iron in aqueous cupric ammine solutions. ISIJ International, 36(5), 522–527. https://doi.org/10.2355/isijinternational.36.522
  11. Yoo, K., Park, Y., Choi, S., & Park, I. (2020). Improvement of copper metal leaching in sulfuric acid solution by simultaneous use of oxygen and cupric ions. Metals, 10(6), 721. https://doi.org/10.3390/met10060721
  12. Zhou, P., Hutchison, M. J., Erning, J. W., Scully, J. R., & Ogle, K. (2017). An in situ kinetic study of brass dezincification and corrosion. Electrochimica Acta, 229, 141–154. https://doi.org/10.1016/j.electacta.2017.01.078

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.