Washing longer or changing the cleaner is the usual response when washed parts fail cleanliness inspection, but without knowing what contamination caused the fail and where it came from, more washing may leave the result unchanged. What actually lies behind it can be washing aimed without telling particles from oil film, recontamination during drying and handling, particles returning from poorly filtered wash fluid, contamination from packaging, or variation in the test method, and sometimes two or more at once.

Background

A few parts fresh from the washer go to the cleanliness lab, and the verdict comes back as a fail: the weight of particles left on the analysis filter, or the length of the largest particle, is over the limit. The lot is held from shipment, the line and its people are tied up while it is rewashed or sorted part by part, and if the customer's incoming inspection caught it, a claim and extra testing follow. Such inspections exist because particles left on a part can, once it is assembled, impair the function that part serves (VDA, 2025).

A component cleanliness inspection usually runs as extraction, washing particles off the part surface into a liquid; filtration, passing that liquid through an analysis filter; and analysis, weighing the particles collected on the filter or sizing and counting them under a microscope. The international standard sets pressure rinsing, ultrasonics, agitation and internal rinsing as extraction methods, and gravimetric and light-optical analysis among the analysis methods (ISO, 2018). The automotive guideline covering the same ground states that this particle inspection does not deal with film-type contamination such as oils, anti-corrosion agents, hand sweat and fluid residues, or with ionic contamination (VDA, 2025).

So a single fail verdict can arise along several paths. Washing may not have removed that contamination; particles it removed may have come back via the wash fluid; the cleaned part may have picked up dirt again during drying, handling or packing; or the measurement itself may have produced a different value. Washing for longer addresses only the first of these.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: confirm from the fail report which criterion was exceeded, whether particle weight, counts per size class or the largest particle, then gather the filter images and the inspection specification and compare them with the customer's cleanliness specification, the wash process settings and the cleaner's technical data sheet, the TDS.

Hypothesis 1: particles vs film

When a part fails cleanliness, some plants first raise the cleaner's concentration and temperature. But if what failed is large metal particles such as machining chips or burr fragments in blind holes, pushing the chemistry harder changes little, and the reverse also happens: pressure is raised when the real issue is leftover oil film. Consider a machined valve housing. A stronger degreaser cut the surface oil, but the next inspection still fails on a few metallic chips that seem to have come from inside the cross-drillings.

Particles and oil film hold on in different ways and need different forces to come off. Particles are held to the surface by intermolecular attraction, capillary forces from moisture and electrostatic forces, and removing them takes a force such as flow or vibration that exceeds these (Visser, 1995). In research on removing particles by flow, particles came off only when the particle Reynolds number, set by particle size and the local flow strength, exceeded a critical value, and since this number shrinks with particle size, smaller particles need stronger flow (Burdick et al., 2001). Oil film is removed by the cleaner dissolving or emulsifying it, so concentration and temperature matter there. They are measured separately as well. The standard for product cleanliness levels sets particle levels and levels of nonvolatile residue, the film-type residue, separately and has them stated together (IEST, 2013).

Look for clues in the filter images. Whether metallic-looking fragments, fibres or dull grains dominate tells which particles drove the fail, and metallic shine is a good indication that a particle came from metal, though it is an optical classification that a person must double-check (VDA, 2025). Oil film does not show up in a particle inspection, so check it separately. The water-break test, pouring clean water over a freshly washed part and watching whether the film of water breaks, is a quick screen for hydrophobic films on the surface (ASTM International, 2021).

If metal particles are the failing item, direct the cleaning's mechanical force to where they sit. Aim nozzles into blind and intersecting holes or use through-flow cleaning, and make sure burrs come off in the upstream process. If oil film is the problem, set the cleaner type, concentration and temperature within the TDS range and check the rinse. Either way, first confirm in writing what the customer specification requires, and how much, of particles and of film.

Hypothesis 2: recontamination

Look at recontamination when the washer exit opens into the same space as machining, when wet parts wait on open conveyors or benches to dry, when shop compressed air blows off the water, or when parts are moved by bare or cotton-gloved hands. A common picture: parts from the washer are lined up on a roller conveyor next to the machining centres, an operator blows water out of the holes with a shop air gun, and the parts go to the lab in a plastic box used elsewhere in the plant.

A cleaned surface starts taking up surrounding particles again from that moment. Particles settling on a wet surface are held firmly by the capillary forces the moisture creates, and on a surface rubbed against plastic boxes or gloves, electrostatic forces pull particles in (Visser, 1995). Nor is the air clean. Cleanrooms are classed by airborne particle concentration because ordinary plant air carries particles, and the automotive guideline notes that fibres are particularly pervasive in ordinary air and present even in cleanrooms (ISO, 2015; VDA, 2025). Compressed air can carry particles, water and oil, and the international standard sets compressed air purity classes for these three (ISO, 2010).

Recontamination shows itself when measured station by station. From the same lot, pull one part each straight after the washer, after drying and just before packing, and test them the same way. If the part straight after the washer passes and values climb further down the line, the steps in between are the cause. Look at the particle types on the filter as well. More fibres and dust point to the air and gloves; more metal particles like the machining chips point to the machining area. On the compressed air line, check the state of the filters and drains.

Once the station is identified, make the route after washing short and clean. Partition the washer exit and drying area from machining, use filtered air for drying, and use only clean gloves and designated containers. Cut the time washed parts spend waiting in the open as well. The automotive industry has a separate guideline on particles introduced in assembly by environment, logistics, people and equipment, which can serve as the reference for such measures (VDA, 2010).

Hypothesis 3: poor filtration

This hypothesis is strong for recirculating washers that collect fluid in a tank and spray it again, where filters have a coarse rating, when a filter is clogged and its bypass valve is open, or when fluid changes and tank bottom cleaning are overdue. Machines that do the final rinse with water from the same tank as an earlier stage belong here too. On Monday the fluid is changed and the tank cleaned, and that day's inspections come out well; towards the weekend, particle weight climbs for the same parts under the same settings.

Particles removed by washing do not disappear; they move into the wash fluid. If filtration does not take them out, the pump and nozzles spray them back onto the next parts with the fluid, and particles left in the final rinse water stay on the surface as the part dries. A filter's rating is not a boundary that stops every particle of a given size. The multi-pass test that measures filtration performance expresses it as the ratio of particle counts upstream and downstream of the filter for each size (ISO, 2022), so some particles of the stated size pass through any filter. An open bypass around a clogged filter lets particles straight through.

Look for the answer in the wash fluid. Take samples at fixed intervals near the spray nozzles and in the final rinse tank, count the particles, and record them with the code used for solid particle contamination in hydraulic fluids, so that changes over the days can be seen at a glance (ISO, 2021). Overlay those values on the part inspection results and the days since the last fluid change. Check the pressure difference across the filters, any sign that a bypass valve has opened, and whether the filter rating suits the particle sizes in the part specification.

If the wash fluid looks to be the cause, rework the filtration. Fit a finer filter on the final rinse than on earlier stages, arrange piping and flow so the whole volume passes through filtration, and change filters on pressure difference. Base fluid changes and the removal of chips and sludge from the tank bottom on the particle count in the fluid rather than on the calendar.

Hypothesis 4: dirty packaging

Look at packaging when parts go straight into cardboard boxes or use paper dividers, when returned plastic trays are reused unwashed, when foam or other cushioning touches the parts, or when several parts go loose into one bag. An example: a lot that passed in-house fails the customer's incoming inspection, and the filter images the customer sends are full of paper fibres and dull grains.

Packaging is the surface a part touches longest after washing. For the packaging that carries inspected parts to the lab, the automotive guideline states that cardboard is unsuitable in direct contact with parts because it generates large quantities of particles, that films and bags touching parts must be clean and unused, and that reusable packaging in which parts are placed directly must be cleaned before use. The same guideline notes that when several parts move loose inside one pack, they strike and rub against each other in transport and shed particles, and that particles falling from parts in transit can collect inside the packaging. It adds that these criteria cannot simply be applied to reusable series packaging (VDA, 2025), but cardboard sheds particles and parts rubbing together shed metal in shipping packaging just the same.

Measure before and after packing side by side. Inspect a part pulled just before packing and parts from the same lot that were packed, held for the real transit time and then unpacked, using the same method, and rinse the inside of the packaging to look at its particles too. If only the packed parts rise and the filter shows paper fibres, bits of cushioning, plastic shavings or metal dust from parts rubbing together, packaging is the cause. For reusable trays, check whether there is a cleaning record and when they were last washed.

Once it narrows to packaging, start with the surfaces that touch the parts. Keep cardboard and paper out of direct contact, use clean new bags or washed trays, and give each part its own slot or divider so parts do not knock together. Agree the cleaning interval and responsibility for reusable packaging with the customer in writing.

Hypothesis 5: test variation

Suspect the measurement first when the in-house and customer labs use different extraction methods or analysis equipment, when the inspector has changed, when results for the same part swing widely from day to day, or when blank values are not measured. It can happen that in-house the part is extracted by manual pressure rinsing and judged a pass, while the customer extracts it by ultrasonics, analyses it on different equipment and reports a fail. Each side believes its own result.

A cleanliness value is defined together with its test method. Since there are no reference parts carrying a known level of contamination, the automotive guideline has the extraction method qualified first for each part by a declining test, extracting the same part repeatedly to see whether the last value falls below 10% of the total extracted so far. Contamination added by the inspection itself is measured as a blank value and kept within a criterion. The guideline regards manual pressure rinsing as making low blank values hard to reach, because of its large wetted area, and as strongly influenced by the inspector, while ultrasonic extraction is reliably reproducible with little inspector influence. It also states that light-optical and scanning electron microscope analysis use different contrast mechanisms, so their particle counts cannot be compared with each other (VDA, 2025).

Write the two labs' inspection specifications side by side on one sheet. Check whether extraction method and liquid, liquid volume, pressure or ultrasonic settings, extraction time, analysis filter pore size, analysis method and size classes, and image brightness and threshold settings are the same. Check that blank value records and declining test records exist. Then split parts from one lot and test them in both labs, and where possible re-analyse a filter from one lab on the other lab's equipment, to separate differences arising in extraction from those arising in analysis.

If it turns out to be a measurement difference, align one inspection specification with the customer. Qualify the extraction method by declining test, measure and record blank values regularly, and repeat side-by-side comparisons on the same parts at intervals. Do not change the wash process before the specification is aligned, since the effect of a process change cannot be judged while the measurement is unsettled.

Finding the cause

There is no need to search all five hypotheses at once. The fail report, filter images and the two labs' specifications are already to hand, so begin with the measurement and the type of contamination. Knowing which criterion was exceeded and what kind of particles sit on the filter decides which of the remaining hypotheses to look at first.

Next comes station-by-station testing. From one lot, measure one part each straight after the washer, after drying, just before packing, and after packing and holding for the transit time, all by the same method. A fail straight after the washer points to the wash itself or to wash fluid filtration; a pass at the washer with values climbing after drying or handling points to recontamination; a rise only after packing points to packaging. If only the gap between in-house and customer results is large, look at the test method and the transport packaging together.

The shape of the particles also points somewhere. Metallic-looking particles such as machining chips and burr fragments may mean too little mechanical force in the wash or fluid spraying them back, while fibres and paper fragments point to air, gloves and packaging. Values that climb day by day after a fluid change point to filtration, and values for the same part that vary with the inspector or the lab point to the measurement.

If that still does not settle it, run control tests. Compare parts washed in freshly changed fluid with parts washed in old fluid, parts in clean new bags with parts in the usual packaging, and parts from one lot measured by the in-house and the customer methods. Change only one thing at a time, or there is no telling what made the difference. Confirm the fix by measuring several consecutive lots by the customer specification's method and seeing whether the passes hold.

The hypotheses can overlap. When parts from a poorly filtered washer dry in the open and go into cardboard boxes, contamination from three places adds up in one result. In such cases, settle the measurement first, then get the value straight after the washer to a pass, and only then work down the later steps in order. While the measurement is unsettled or the upstream step already fails, there is no judging whether measures further down the line worked.

Limits and cautions

Permitted particle size, count and weight, limits for film residue, and extraction and analysis conditions depend on the part's function and the customer specification, so numeric decisions follow the cleanliness and inspection specifications agreed with the customer and the cleaner's TDS. Which particles harm function is for design and quality engineers to judge, and before any major change to the wash process, check whether the customer has an approval procedure for it.

Safety matters too. For cleaners and extraction solvents, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and keep flammable solvents away from flames and static. When blowing parts off with compressed air, wear eye protection against flying particles and liquid, and never point the air at the body. Inspect washer pumps, tanks and filters only after the machine is stopped and locked out.

Sources

  1. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  2. Burdick, G. M., Berman, N. S., & Beaudoin, S. P. (2001). Describing hydrodynamic particle removal from surfaces using the particle Reynolds number. Journal of Nanoparticle Research, 3(5–6), 453–465. https://doi.org/10.1023/A:1012593318108
  3. Institute of Environmental Sciences and Technology [IEST]. (2013). IEST-STD-CC1246E, Product cleanliness levels: Applications, requirements, and determination.
  4. International Organization for Standardization [ISO]. (2010). ISO 8573-1:2010, Compressed air — Part 1: Contaminants and purity classes. https://www.iso.org/standard/46418.html
  5. International Organization for Standardization [ISO]. (2015). ISO 14644-1:2015, Cleanrooms and associated controlled environments — Part 1: Classification of air cleanliness by particle concentration. https://www.iso.org/standard/53394.html
  6. International Organization for Standardization [ISO]. (2018). ISO 16232:2018, Road vehicles — Cleanliness of components and systems. https://www.iso.org/standard/70267.html
  7. International Organization for Standardization [ISO]. (2021). ISO 4406:2021, Hydraulic fluid power — Fluids — Method for coding the level of contamination by solid particles. https://www.iso.org/standard/79716.html
  8. International Organization for Standardization [ISO]. (2022). ISO 16889:2022, Hydraulic fluid power — Filters — Multi-pass method for evaluating filtration performance of a filter element. https://www.iso.org/standard/77245.html
  9. Verband der Automobilindustrie [VDA]. (2010). VDA 19.2, Technical cleanliness in assembly: Environment, logistics, personnel and assembly equipment. https://webshop.vda.de/QMC/en/Volume-192
  10. Verband der Automobilindustrie [VDA]. (2025). VDA 19.1, Inspection of technical cleanliness: Particulate contamination of functionally relevant automotive components (3rd rev. ed.). https://vda-qmc.de/wp-content/uploads/2025/07/VDA-19.1_Yellow-Volume_2025_EN.pdf
  11. Visser, J. (1995). Particle adhesion and removal: A review. Particulate Science and Technology, 13(3–4), 169–196. https://doi.org/10.1080/02726359508906677

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.