KALTECKOREA

BlogApplication notes

Why do aluminium parts corrode in an equipment cooling loop topped up with water?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Heat Transfer & Cooling

Replacing the part and refilling with water is the usual response to corroded aluminium parts, but as long as the same water keeps meeting the same metals, the new part tends to go the same way. What actually lies behind it can be water with no inhibitor, copper plating out on the aluminium, pH out of range, chloride building up with each top-up, microbes growing in the loop or oxygen that keeps getting in, and sometimes two or more at once.

Background

When the level alarm on the chiller next to a machine goes off, someone fills a container from the tap, pours it into the tank, and the alarm clears. A few months of that, and water starts to weep from a joint on an aluminium cold plate; opened up, its channels show white powder and small holes. The coolant has turned cloudy, and grey sludge sits in the filter.

Corrosion in a cooling loop is more than one part's problem. Leaking water stops the machine and can reach nearby electrical parts, and corrosion products block narrow channels and filters, cutting cooling performance. As corrosion builds up it weakens the metal, leading to equipment damage, lost efficiency and higher maintenance costs (NIH, 2023).

Aluminium is a reactive metal, but a thin oxide film on its surface lets it survive in water. The film is stable near neutral pH but dissolves on the acid and alkaline sides (Pourbaix, 1974; Vargel, 2004). When the film breaks at only a few points, those points are eaten deep, which is pitting, and the solution inside a narrow pit turns acidic, unlike the water outside, so the pit keeps growing on its own (Frankel, 1998). Solving aluminium corrosion therefore means looking both at what breaks the film and at what keeps the reaction going where it broke.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: list the metals in the loop as aluminium, copper, brass, steel and stainless steel, gather the dates and volumes of every top-up, and take samples of loop water and top-up water on the same day to compare side by side.

Hypothesis 1: no inhibitor

This hypothesis covers loops filled with tap or pure water from the start, loops topped up with water only by people who never knew what coolant came with the machine, and loops that once held inhibitor but have been diluted by top-up after top-up. Two or three years after installation, no one remembers the original coolant specification. Water from the nearest tap has gone in every time the level alarm sounded, and the coolant has grown paler each year. A thin layer of white sediment covers the tank floor.

An inhibitor is a chemical that heads off the attacks that break the film. Aluminium alloys contain small regions rich in iron or silicon, and the film around them is weak and tends to become a local cathode. In hot aqueous tests, adding an inhibitor formed a thin silicon dioxide layer on the surface that stopped copper from depositing, and corrosion in copper-ion solution fell sharply (Chiba et al., 2014). Blends of nitrite, molybdate and azole are used to protect loops that mix steel, copper and aluminium (NIH, 2025). Of these, azoles adsorb on copper and form a film that reduces copper dissolving into the water (Finšgar & Milošev, 2010). A loop holding only water lacks every one of these defences.

Coolant colour does not show whether inhibitor remains, so measure the inhibitor components with the supplier's test kit or in a laboratory. If the original coolant is unknown, start by having the water analysed for nitrite, molybdate, azole and silicate. Look at the top-up records too. A closed loop normally needs make-up of less than 5% of its volume a year, yet losing 25% a month through small mechanical seal leaks or expansion tank overflow is not uncommon (NIH, 2023). If the water added has exceeded the loop volume several times over, assume little of the original inhibitor is left.

If the inhibitor has run out, the first step is choosing one that suits the loop's metals, and the supplier must be told that aluminium is present. Remove corrosion products and sediment by cleaning and flushing, then refill. Top up with coolant mixed to the same strength rather than plain water, or add inhibitor with every top-up to hold the concentration. Logging top-up volumes and inhibitor levels in the same record lets the next change show early.

Hypothesis 2: copper plating out

Suspect copper when copper pipe, a chiller heat exchanger with copper tubes or brass fittings share water with aluminium cold plates or an aluminium heat exchanger. Watch more closely when only water circulates with no azole, right after new copper pipe is joined in, and when a lot of oxygen is dissolved. Picture opening up a corroded aluminium cold plate. Reddish-brown dots are embedded here and there on the channel walls, each ringed by a white swelling. On the far side of the same loop sits a chiller with a copper-tube heat exchanger.

The water connects the two metals even when they never touch. Copper ions dissolved from the copper side travel with the water to the aluminium surface, where aluminium gives up electrons and dissolves while copper settles out as metal in its place. The deposited copper particles act as local cathodes that keep dissolving the aluminium around them, and with chloride present copper deposited over wider areas and corrosion became far more severe (Chiba et al., 2014). Heavy-metal ions such as copper are counted among the main triggers of pitting in aluminium (Vargel, 2004).

Measure copper in the loop water alongside the top-up water. Iron and copper above top-up levels signal that parts in the loop are corroding now (NIH, 2025). If an aluminium part can be removed, look around the pits under a magnifier for red metallic dots, and if needed send it for surface analysis to see whether copper sits inside the pits. Trace on the loop drawing whether copper and aluminium share the same water.

Where copper deposition shows, change the water first. Dissolved copper does not filter out, so drain and rinse the loop, then refill with a mixed-metal inhibitor containing azole so that copper stops dissolving again. Breaking direct metal contact at joints with insulating fittings helps, but it cannot stop copper ions carried by the water. When selecting equipment or modifying the loop, review with the equipment supplier whether aluminium and copper can be put on separate water circuits.

Hypothesis 3: pH out of range

Look at pH when a treatment set high for steel pipe is used unchanged, when the loop is filled with softened water, and when rinsing was cut short after an alkaline or acid cleaner. Suppose the loop was cleaned with an alkaline cleaner at a scheduled service, rinsed briefly and refilled. A few weeks later an aluminium fitting is opened: its inner face is roughened all over rather than pitted, and translucent, gel-like sediment floats in the coolant.

Aluminium oxide is amphoteric, so it dissolves in both acid and alkali. It goes into solution as aluminium ions on the acid side and as aluminate ions on the alkaline side, so the film protects only within a narrow pH band between them (Pourbaix, 1974). Attack of this kind often wears a wide area down evenly rather than forming pits. The German guideline for heating water lowers the upper pH limit from 10.0 to 9.0 where water touches aluminium, and recommends demineralisation rather than softening for systems containing aluminium (VDI, 2021). Closed loops of steel pipe are advised to run at pH 9.0 to 10.5 (NIH, 2025), so carrying a steel-based treatment over to a loop that includes aluminium can leave the pH too high for the aluminium.

Measure loop water and top-up water together with a calibrated pH meter, reading the samples on the spot. A trend over several weeks says more than a single value, so check against the records how pH moved after cleaning or a water change. Look in the work records for whether softened water is used and whether the pH of the rinse water was checked after cleaning.

If the loop contains aluminium, set the pH target within the range the equipment supplier and the inhibitor's TDS allow for aluminium. After a cleaner, rinse until the rinse water's pH matches the top-up water, and consider demineralised rather than softened water for filling and topping up. Rather than pouring acid or alkali straight in to correct pH, an inhibitor containing a buffer lets the pH hold itself, with less swing.

Hypothesis 4: chloride build-up

Chloride tends to build up in loops topped up with groundwater or tap water, loops where water evaporates from an open tank and top-ups are frequent, and loops once disinfected with chlorine-based products. When water leaves by evaporation, the salts dissolved in it stay behind, so every top-up adds more salt. Consider a plant that filled an open-tank chiller nearly every day through the summer. By autumn, pinhole leaks have appeared at a few spots on the aluminium cold plates, each capped by a small white lump like a blister.

Chloride ions attach to weak spots in the oxide film and break it locally. Aluminium ions released at the break react with water to make acid, chloride gathers into the pit to keep the charge balanced, and the inside of the pit becomes a concentrated acidic chloride solution. That solution keeps the film from healing, so the pit deepens while white aluminium hydroxide piles up at its mouth (Szklarska-Smialowska, 1999). In hot aqueous tests too, chloride destabilised the film at iron- and silicon-rich spots and increased corrosion (Chiba et al., 2014).

Measuring chloride in loop water and top-up water side by side shows at once whether chloride has built up. Record electrical conductivity as well. High conductivity without inhibitor raises the risk of localised corrosion, and chloride and sulphate drive pitting and crevice corrosion (NIH, 2025). Loop water several times stronger than top-up water means salts are building up by evaporation; similar values mean the top-up water itself is bringing chloride in.

Once chloride has built up, draining the concentrated water and refilling is about the only way to bring it down. Use low-salt demineralised water for refilling and topping up, and cover open tanks to cut evaporation. If the loop must be disinfected, choose a biocide suited to the inhibitor and to aluminium with the supplier instead of a chlorine-based product. Setting replacement limits for chloride and conductivity heads off a repeat.

Hypothesis 5: microbial growth

Microbes settle easily in idle equipment, blind branch lines where water stands, loops that run lukewarm and loops topped up often with untreated water. It is the day a machine restarts after a two-week holiday shutdown. The filter is clogged with sticky brown lumps, and opening the tank lid releases a smell of rotten eggs.

Top-up water brings microbes and organic matter in with it, and stagnant branches are especially easy places for them to grow. Nitrite, a common inhibitor in closed loops, can even feed some bacteria (NIH, 2023). Microbes build a biofilm on the metal, and the water beneath it differs in oxygen and composition from the bulk, so localised corrosion can start under the film. Iron sulphide deposits and acidic by-products are read as signs of microbial activity (NIH, 2025). How far microbes took part in a given corrosion case, however, cannot be settled by one test and needs several lines of evidence together (Little et al., 2020).

When microbes are suspected, take samples in sterile containers where water stands still, at blind branches and low-flow points. Use dip slides for general bacteria, ATP measurement for overall microbial activity, and dedicated culture tests for specific groups such as sulphate-reducing bacteria (NIH, 2025). Note the smell and colour of the filter sludge and any black deposit at corrosion sites as well.

If bacterial counts come back high, the biofilm has to be removed before a biocide can work. Clean and flush the loop, then agree with the supplier on a biocide that can be used with the inhibitor and does not harm aluminium. Remove unused branch lines, and keep water moving now and then during long shutdowns to cut stagnant zones. If the top-up source has changed, check its bacterial count once as well.

Hypothesis 6: oxygen ingress

Open tanks in contact with air, frequent top-ups with aerated water, small leaks at joints on the pump suction side, plastic hoses that let oxygen through and high pipe runs at low pressure are all routes for oxygen. On one machine, a loose joint on the pump suction side hisses, and strings of small bubbles flow through a clear hose. The tank surface is always covered in froth, and the top-up interval keeps getting shorter.

Oxygen handles the other half of the corrosion reaction. Dissolved oxygen is what takes up the electrons aluminium releases as it dissolves, so a steady supply keeps local cathodes such as deposited copper or iron- and silicon-rich spots working without a break (Frankel, 1998). Even in a closed loop, dissolved oxygen keeps getting in through top-up water and leaks and drives corrosion (NIH, 2023). For heating pipework made of plastic, there is even a standard requiring a barrier layer against oxygen diffusing through the pipe wall (DIN, 2024).

Find the routes in by eye and ear first. Look for bubbles, froth and noise at suction-side joints, and check with a pressure gauge that the highest point of the loop stays above atmospheric pressure. Measure dissolved oxygen in loop water and top-up water with a dissolved-oxygen meter, comparing readings near the tank and far from it. A shrinking top-up interval means the leak is also a route for oxygen, so read the top-up records alongside.

Proper pressurisation and keeping flushing to a minimum are named as the keys to stopping air ingress (NIH, 2025). Retighten suction-side joints or replace their seals so no air is drawn in, and consider changing open tanks for sealed or covered ones. Replace plastic hoses with types that have an oxygen barrier, and set the fill pressure so the high points of the loop stay pressurised. Where oxygen cannot be kept out completely, review with the supplier an oxygen scavenger that works alongside the inhibitor.

Finding the cause

Four of the six hypotheses narrow a great deal with a single round of water samples. Take loop water and top-up water on the same day and measure pH, conductivity, chloride, copper and inhibitor side by side; that shows together whether the inhibitor is gone, whether copper is circulating, whether pH has left the range for aluminium and whether chloride has built up. Microbes and oxygen come after that, with samples from stagnant points and measurements on site.

The shape of the corrosion is a clue too. A wide area worn down evenly with no pits points to pH that has strayed to the acid or alkaline side. Red metallic dots around pits point to copper deposition, while many pinholes capped with white blisters and no red dots point first to chloride and missing inhibitor. Sticky sludge with a rotten-egg smell points to microbes, and visible bubbles with frequent top-ups point to oxygen ingress.

To compare before and after a water change in numbers, hang aluminium coupons in the loop. A standard test exposes metal coupons in a side-stream rack for a set period and then assesses weight loss and pitting; exposing the same metal to different waters compares how corrosive they are, and the method is also used to test inhibitor effect (ASTM International, 2023). Match the coupon alloy to the aluminium parts in the loop, and hang a copper coupon alongside to see whether copper is dissolving.

Make control changes one at a time. First drain, rinse and refill with a suitable inhibitor, then close off the oxygen routes, and finally bring microbes under control. After each change, log copper, chloride and inhibitor in the loop water and the coupon results on the same basis, and treat the job as done only once those values hold steady.

The hypotheses often arrive together. Copper and chloride together make corrosion far worse than either alone (Chiba et al., 2014), and oxygen that keeps coming in stops the reaction from ever slowing. A loop topped up with plain water dilutes its inhibitor while taking in chloride, oxygen and microbes at the same time, so the usual course is to put the water chemistry right first and then turn to oxygen and microbes. While the water is unsettled, the effect of any other measure is hard to judge.

Limits and cautions

Suitable pH, inhibitor strength and limits for chloride and conductivity vary with the loop's metals, temperature and equipment, so numeric decisions follow the equipment supplier's coolant specification and the inhibitor's TDS. The German guideline's pH range cited above was written for heating systems and serves only as a reference for equipment cooling loops. For equipment such as semiconductor or laser tools, where the coolant carries electrical requirements too, the equipment supplier's specification comes first, and adding an inhibitor may not be allowed at all.

For cleaners, inhibitors and biocides, follow each product's safety data sheet, the SDS, for protective equipment and ventilation, and check with the supplier before mixing different chemicals. Where electrical parts sit near a coolant leak, isolate and lock out the power before working. Parts that keep leaking, heat exchangers under high pressure and parts that carry structural load should not stay in service on floor judgement alone; have the equipment supplier inspect them.

Sources

  1. ASTM International. (2023). ASTM D2688-23, Standard test method for determination of corrosion rate in a water system. https://store.astm.org/d2688-23.html
  2. Chiba, M., Nakayama, Y., Hiraga, T., Saito, S., Shibata, Y., & Takahashi, H. (2014). Corrosion of aluminum alloys in hot aqueous solutions and dry/wet-repeating atmospheres: Effects of the concentration of Cl−, Cu2+, and dissolved O2, and of the addition of an inhibitor. Corrosion Engineering, 63(8), 449–458. https://doi.org/10.3323/jcorr.63.449
  3. Deutsches Institut für Normung [DIN]. (2024). DIN 4726:2024-12, Warm water surface heating systems and radiator connections – Plastics and multilayer piping systems. DIN Media. https://www.din.de/en/wdc-beuth:din21:380677149
  4. Finšgar, M., & Milošev, I. (2010). Inhibition of copper corrosion by 1,2,3-benzotriazole: A review. Corrosion Science, 52(9), 2737–2749. https://doi.org/10.1016/j.corsci.2010.05.002
  5. Frankel, G. S. (1998). Pitting corrosion of metals: A review of the critical factors. Journal of the Electrochemical Society, 145(6), 2186–2198. https://doi.org/10.1149/1.1838615
  6. Little, B. J., Blackwood, D. J., Hinks, J., Lauro, F. M., Marsili, E., Okamoto, A., Rice, S. A., Wade, S. A., & Flemming, H.-C. (2020). Microbially influenced corrosion—Any progress? Corrosion Science, 170, 108641. https://doi.org/10.1016/j.corsci.2020.108641
  7. National Institutes of Health [NIH]. (2023). Closed-loop systems water treatment (Technical Bulletin No. 135). Office of Research Facilities. https://orf.od.nih.gov/TechnicalResources/Documents/Technical%20Bulletins/23TB/Closed%20Loop%20Water%20Treatment%20-%20August%202023%20Technical%20Bulletin_508.pdf
  8. National Institutes of Health [NIH]. (2025). Corrosion in closed loop water systems part 2: Evaluation and prevention (Technical Bulletin No. 152). Office of Research Facilities. https://orf.od.nih.gov/TechnicalResources/Documents/Technical%20Bulletins/25TB/Corrosion%20in%20Closed%20Loop%20Water%20Systems%20Part%202%20-%20Evaluation%20and%20Prevention%20-%20June%202025%20TB_508.pdf
  9. Pourbaix, M. (1974). Atlas of electrochemical equilibria in aqueous solutions (2nd English ed.). National Association of Corrosion Engineers.
  10. Szklarska-Smialowska, Z. (1999). Pitting corrosion of aluminum. Corrosion Science, 41(9), 1743–1767. https://doi.org/10.1016/S0010-938X(99)00012-8
  11. Vargel, C. (2004). Corrosion of aluminium. Elsevier.
  12. Verein Deutscher Ingenieure [VDI]. (2021). VDI 2035 Part 1, Prevention of damage in water heating installations – Scale formation and water-side corrosion.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.