Switching to a stronger adhesive is the usual response to weak composite bonds, but if the adhesive never properly attached to the composite surface and lets go at the interface, a new adhesive will not bring the strength back. What actually lies behind it can be release agent residue, inadequate surface preparation, moisture absorbed by the composite, a resin incompatible with the adhesive or the wrong peel ply, and sometimes two or more at once.

Background

Test pieces cut from bonded carbon or glass fibre composite parts come apart at loads far below the standard. On the separated faces, the adhesive sits intact on one side while the composite surface on the other side is bare and smooth. Caught at the test-piece stage, this means rework and retesting; in production parts it means re-inspecting the whole lot, and a failure in service becomes a structural safety issue.

Adhesive attaches to a very thin outer layer of the composite surface. So the same adhesive can give very different results depending on what sits on that outer layer and how well the adhesive wets it. The way a joint fails is an important clue. Unlike cohesive failure, where the adhesive layer or the composite itself tears, interfacial failure, where adhesive and surface separate, gives strength that is not only low but hard to predict, and the lap shear test shows only short-term strength and says little about durability (Guin et al., 2023).

The causes of weak composite bonds mostly lie in the steps before the adhesive rather than in the adhesive itself. Contamination carried over from moulding, an under-prepared surface, water held in the composite, a matrix resin that does not suit the adhesive and the peel ply that formed the surface all change the outer layer the adhesive has to grip.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep both separated faces and record on which face and how the joint let go, note the release agent and peel ply used in moulding, the surface treatment and the time from treatment to bonding, and the part storage conditions, and compare them with the adhesive's technical data sheet, the TDS, and the process standard.

Hypothesis 1: release agent residue

Composites cure against moulds coated with release agent or on release films so that they come off cleanly, so release agent can always transfer to the surface to be bonded. Look at this hypothesis when the tool side is bonded as it is, when parts come from a mould just after fresh release agent was applied, and when bonding takes place near work areas that use silicone-based release agents or lubricant sprays. Picture the first few panels pulled after mould maintenance. The surface is glossy and looks clean, and it was even wiped once with solvent, yet only test pieces from these panels fail at low load, with almost no adhesive left on the separated face.

Release agents are made so that nothing sticks to them, and left on a bonding surface they push the adhesive away exactly as designed. The adhesive either fails to wet the release film or cures sitting on top of it, and under load the joint separates at the interface along the release layer. In a study of carbon fibre composite joints contaminated with a silicone-based release agent, fracture toughness fell sharply once silicon on the surface exceeded 5 atomic percent, and above 7 atomic percent no adhesion formed at all (Markatos et al., 2014). One aerospace research facility that tested composite bonds monitored airborne silicone in the workshop regularly and placed a sacrificial layer between the released tool face and the bonding surface so that release agent could not transfer (Guin et al., 2023).

Release agent cannot be seen by eye, so check with water. The water-break test, in which clean water is run over the bonding surface to see whether it stays as an even, continuous film or breaks into droplets, is set out as a standard test method (ASTM International, 2021). If the breaks cluster on tool-side faces or on parts from a particular mould, the evidence leans towards release agent. If the separated face is smooth with no adhesive left on it, send it to a laboratory to measure release agent elements such as silicon or fluorine by X-ray photoelectron spectroscopy, or XPS.

With release agent confirmed, cut off the route by which it transfers. Co-cure a sacrificial layer such as a peel ply on surfaces to be bonded so release agent never reaches them, and where that is not possible, do not stop at a solvent wipe; abrade away the outer layer and then wipe again. Run freshly released moulds through the number of blank cycles the supplier specifies before production, and keep silicone sprays and release agents out of the bonding area. Adding the water-break test as a check just before bonding catches the problem early if it returns.

Hypothesis 2: poor surface prep

If bonds are weak with no release agent present, check whether surface preparation fell short. That applies when abrasion was skipped and the surface only wiped with solvent, when it was abraded but the dust not removed, when a long time passed between plasma treatment and bonding, and when the treated surface was handled with bare hands. On a busy day, an operator moves freshly abraded and wiped parts onto the jig bare-handed. Parts handled with gloves on other days exceed the standard, while test pieces from that day's batch are weaker and their separated faces are uneven.

Surface treatment removes or chemically changes the composite's outer layer to give the adhesive somewhere to wet and grip. Physical treatments such as abrasion and solvent wiping are set out in a standard practice as ways to remove the glossy outer layer and contaminants (ASTM International, 2025). The chemical side works like this. In a study that treated aerospace glass and carbon fibre epoxy composites with atmospheric pressure plasma to overcome the low surface energy of the polymer matrix, fluorine disappeared from the surface while oxygen and nitrogen were added, giving a surface that water wetted more readily, and all double cantilever beam specimens failed cohesively inside the composite (Encinas et al., 2014). In another study, strength rose with the number of plasma passes to as much as 50% above untreated specimens, and the gain tracked the carboxyl groups that built up on the surface (Zaldivar et al., 2010).

What to check is the treatment record and wetting. Match the abrasion method and grit, the solvent used and the times of treatment and bonding part by part, and see whether weak test pieces cluster in batches that waited long after treatment, with a particular operator or with a particular abrasive. Measure wetting on the treated surface with the water-break test or water drop contact angle and compare readings straight after treatment and a few hours later; whether activity fades with time then shows in numbers. If the separated face shows patches of shiny original surface, those are spots the abrasion did not reach.

If surface preparation is the cause, pin the procedure down in numbers. Abrade until the gloss is gone evenly, lift the dust off with a dry cloth, then wipe with clean solvent and let it dry, and handle treated surfaces with gloves. Set a maximum time from treatment to bonding, and retreat parts that exceed it. If equipment treatment such as plasma is used, fix the speed, distance and number of passes, and check the effect regularly by contact angle.

Hypothesis 3: absorbed moisture

Moisture becomes a concern when composite parts were stored for a long time in a humid warehouse, when they are bonded straight after water jet cutting or wet machining, in humid seasons such as the rainy season, and when parts from service are repaired. It applies even more when the adhesive is cured at high temperature, as heat-curing adhesives are. Panels stacked in a warehouse with the doors open through the summer rains are taken out in autumn and bonded with a heat-curing film adhesive. Test pieces come out weaker than those bonded in spring straight after the same panels were made, and the cross-section of the separated adhesive layer is dotted with small pores.

Epoxy-based composites slowly take up moisture from the air. When such a composite is heated to cure the adhesive, part of the moisture it holds moves into the adhesive, where it can cause heavy voiding, plasticise the adhesive, interfere with cure or weaken the bond between substrate and adhesive (Bond et al., 1998). In the same study, specimens dried before bonding were stronger than undried ones at the same moisture content, and joint strength tracked the amount of moisture that moved from substrate to adhesive. In tests on bonded carbon fibre composites exposed to humidity, fracture toughness under the high-humidity condition was up to 26% lower (Markatos et al., 2014). Carbon fibre composites soaked in water and in water-based machining coolants gained weight, and the specimens soaked in water gave the lowest bond strength (Turner et al., 2015).

Weight is the most reliable evidence. Store small coupons from the same lot alongside the parts, weigh them just before bonding, dry them in an oven and weigh again; the difference is the moisture they held. Match storage time and place and any wet machining against the weak test pieces, and look at the cross-section of the separated adhesive layer under a magnifier for clustered pores. Splitting the same parts into dried and undried sets and bonding both shows moisture's share most clearly.

With moisture confirmed, build a drying step into the process. For parts that took up moisture in service, as in repair work, a drying procedure is described as necessary before the patch is applied (Budhe et al., 2018). Set drying temperature and time with the part supplier within what the composite resin can tolerate, keep dried parts sealed or in a dry place, and bond them within a set time. Dry wet-machined parts thoroughly before surface treatment, and bring warehouse humidity under control as well.

Hypothesis 4: incompatible resin

If bonds are weak only on certain composites even with proper surface preparation, look at the pairing of matrix resin and adhesive. Give this hypothesis weight when an adhesive used on epoxy composites is applied as it is to composites with a thermoplastic matrix such as polypropylene, polyamide, PPS or PEEK, when the adhesive is cured below the TDS temperature because the part cannot take the heat, and when a change of composite supplier has changed the matrix resin. Take a process applying the usual epoxy adhesive, by the usual procedure, to newly arrived thermoplastic carbon fibre panels. The adhesive cures cleanly, yet the test pieces are weak enough to pull apart by hand and the separated panel faces look untouched.

Thermoplastic-matrix composites have surfaces that repel liquids, which makes them hard to bond, so they need a separate surface treatment to raise wetting. A study comparing aerospace PPS, PEI and PEEK carbon fibre composites found that atmospheric plasma and ultraviolet treatment greatly improved the PEEK and PPS joints, shifting them to cohesive or delamination failure, but had no effect on PEI (Scarselli et al., 2021). Even the same treatment works to different degrees on different resins. Cure temperature is also part of the pairing. In tests that varied process parameters while bonding carbon fibre epoxy composites with a film adhesive, curing the adhesive at too low a temperature was the one parameter that clearly reduced performance, more than time from treatment to bonding or adhesive out-time (Guin et al., 2023).

First confirm what the matrix resin is. Find the resin type and maximum service temperature in the part drawing and the composite supplier's data, and check that the substrates listed in the adhesive's TDS and its cure conditions suit that resin and temperature. Confirm the actual cure temperature from a thermocouple placed near the bond, not from the oven setting. If the separated face is as smooth as the untreated surface with adhesive left only on one side, compare against test pieces bonded to the same resin with a different surface treatment to tell whether the problem lies with the resin.

If the pairing turns out to be wrong, choose adhesive and treatment again to suit the resin. For a thermoplastic matrix, select with the supplier a surface treatment proven on that resin and an adhesive or primer that lists that resin as a substrate. If the part cannot withstand the adhesive's cure temperature, do not force a lower-temperature cure; change to an adhesive that fully cures at a temperature the part can take. Use a new pairing only after confirming cohesive failure on test pieces made under the same conditions as the real part surface.

Hypothesis 5: wrong peel ply

A peel ply is a fabric cured onto the composite surface during moulding and torn off just before bonding, used so that a clean, rough surface appears the moment it is removed. Suspect the peel ply after a change of peel ply type, when nylon and polyester peel plies are mixed in the same process, when a release-treated fabric is used in place of a peel ply, and when parts are bonded straight after peel ply removal without abrasion. From the month purchasing switched to a cheaper peel ply, the failure pattern of bonded test pieces changed. Faces that used to tear away with composite fibres attached now separate as smooth faces carrying the imprint of the fabric weave.

The fabric decides the surface a peel ply leaves. Removing a peel ply changes both the roughness and the elemental composition of the surface, and the peel ply itself can be hard to remove (Thull et al., 2019). Where the fabric fibres are firmly attached to the resin, tearing it off leaves fabric fragments or material carried by the fabric on the surface, and the adhesive then attaches to that leftover layer instead of to the composite. A US Federal Aviation Administration report found that surfaces made with nylon peel ply coated with siloxane and silicone release agents led to interfacial failure and stop-start crack growth, with fracture energy far lower than on surfaces from a PTFE vacuum bag film (Bardis & Kedward, 2001). In the same report, grit-blasted joints had higher failure loads and fracture energy than unblasted ones, but the failure mode, interfacial or cohesive, did not change.

Start by establishing exactly which peel ply is in use. Check in the product data whether the fabric is nylon or polyester and whether it carries a release treatment, and match the date it was introduced against when the weak test pieces appeared. Look at the peeled surface under a magnifier for leftover fabric fibres, and check wetting with the water-break test. If the separated face carries a smooth imprint of the weave, the adhesive let go at the layer the fabric left behind, so have a laboratory check that face for release elements by XPS.

Once the cause is narrowed to the peel ply, choose the fabric again for bonding. Use a peel ply qualified for bonding with no release treatment on surfaces to be bonded, and store release fabrics and peel plies apart so they cannot be mixed up. When changing peel ply type, confirm cohesive failure again with bonded test pieces before production, and use the same tests to decide whether to add light abrasion after peeling. Tear the peel ply off just before bonding so the exposed surface does not pick up contamination again.

Finding the cause

The five hypotheses do not each need testing from scratch. Rule out first what can be read straight from the records and the separated faces. Moulding and surface treatment records, peel ply type and part storage time and place are a matter of paperwork, and a water-break test takes a few minutes on the shop floor. Time-consuming checks such as XPS analysis and drying comparison trials come after that.

The biggest clue is the separated face. If the adhesive layer tore or composite fibres came away with it, the interface held, so look at the adhesive side, such as pores in the layer or a low cure temperature, or at load and design. Adhesive left on one side with a smooth face opposite means an interface problem. If that face is the glossy original surface, suspect release agent or inadequate surface preparation; if it carries a fabric weave imprint, suspect the peel ply. Dense pores in the adhesive cross-section point to moisture held in the composite, and failures confined to parts with a particular matrix resin point to the pairing of resin and adhesive.

If that still does not settle it, run control trials that change one thing at a time. From the same parts, bond sets with and without extra abrasion, dried and undried, and made with the old and the new peel ply, changing only one thing at a time. Compare not only strength figures but also the share of cohesive failure on the separated faces. Interfacial failure gives not only low but widely scattered values, so average strength alone may not reveal the cause (Guin et al., 2023).

The final check is cohesive failure. The job is done only when, after the cause is corrected, test pieces made under the same conditions exceed the standard strength and most of each separated face shows tearing within the adhesive or the composite. For parts where durability matters, add a fracture toughness test or a test after hot-wet exposure to the lap shear test, which shows only short-term strength.

The hypotheses can overlap. A release-treated peel ply is both a peel ply problem and a release agent problem, and even after abrasion removes the release elements, a composite holding moisture can still form pores in the adhesive layer during a heat cure. In such cases, remove contamination first, dry out moisture next, and finally look again at surface treatment and the pairing with the adhesive, because while an earlier step is unsettled, the effect of changing a later one cannot be compared fairly.

Limits and cautions

Suitable abrasion methods, drying temperature and time, time from treatment to bonding and cure temperature differ by composite resin and adhesive, so numeric decisions follow the adhesive's TDS and the composite and peel ply suppliers' guidance. XPS analysis and fracture toughness testing are laboratory work, and for safety-related joints such as structural parts of aircraft or vehicles, do not change the process on floor judgement alone; get approval from the design and quality engineers.

Safety matters too. For adhesives, primers and cleaning solvents, follow the product's safety data sheet, the SDS, for protective equipment and ventilation. Epoxy resins are listed among the main causes of occupational dermatitis, and once skin has become sensitised, a small amount can trigger a severe reaction (HSE, 2022). Collect the dust from abrading or grit blasting composites with extraction, and wear respiratory and eye protection.

Sources

  1. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  2. ASTM International. (2025). ASTM D2093-03(2025), Standard practice for preparation of surfaces of plastics prior to adhesive bonding. https://store.astm.org/d2093-03r25.html
  3. Bardis, J., & Kedward, K. (2001). Effects of surface preparation on long-term durability of composite adhesive bonds (DOT/FAA/AR-01/8). U.S. Federal Aviation Administration. https://rosap.ntl.bts.gov/view/dot/93981
  4. Bond, D., Swan, G., Bader, M., & Smith, P. (1998). The effect of matrix moisture content on the repair of carbon fibre reinforced epoxy. In Proceedings of the 21st Congress of the International Council of the Aeronautical Sciences (ICAS-98-4.4.3). https://www.icas.org/icas_archive/ICAS1998/ABSTRACTS/443.HTM
  5. Budhe, S., Banea, M. D., & de Barros, S. (2018). Bonded repair of composite structures in aerospace application: A review on environmental issues. Applied Adhesion Science, 6(1), 3. https://doi.org/10.1186/s40563-018-0104-5
  6. Encinas, N., Oakley, B. R., Belcher, M. A., Blohowiak, K. Y., Dillingham, R. G., Abenojar, J., & Martínez, M. A. (2014). Surface modification of aircraft used composites for adhesive bonding. International Journal of Adhesion and Adhesives, 50, 157–163. https://doi.org/10.1016/j.ijadhadh.2014.01.004
  7. Guin, W. E., Nettles, A. T., Barnes, B. W., Bausano, J. V., & Opliger, M. S. (2023). A comparison of test methods for the evaluation of bonded joint performance in composite structures (NASA/TP-20230006378). NASA Marshall Space Flight Center. https://ntrs.nasa.gov/citations/20230006378
  8. Health and Safety Executive [HSE]. (2022). Health surveillance for occupational dermatitis (G403). Retrieved November 2026. https://www.hse.gov.uk/pubns/guidance/g403.pdf
  9. Markatos, D. N., Tserpes, K. I., Rau, E., Brune, K., & Pantelakis, S. (2014). Degradation of mode-I fracture toughness of CFRP bonded joints due to release agent and moisture pre-bond contamination. The Journal of Adhesion, 90(2), 156–173. https://doi.org/10.1080/00218464.2013.770720
  10. Scarselli, G., Quan, D., Murphy, N., Deegan, B., Dowling, D., & Ivankovic, A. (2021). Adhesion improvement of thermoplastics-based composites by atmospheric plasma and UV treatments. Applied Composite Materials, 28(1), 71–89. https://doi.org/10.1007/s10443-020-09854-y
  11. Thull, D., Zimmer, F., Hofmann, T., Holtmannspötter, J., Koerwien, T., & Hoffmann, M. (2019). Investigation of fluorine-based release agents for structural adhesive bonding of carbon fibre reinforced plastics. Applied Adhesion Science, 7(1), 2. https://doi.org/10.1186/s40563-019-0117-8
  12. Turner, J., Scaife, R. J., & El-Dessouky, H. M. (2015). Effect of machining coolant on integrity of CFRP composites. Advanced Manufacturing: Polymer & Composites Science, 1(1), 54–60. https://doi.org/10.1179/2055035914Y.0000000008
  13. Zaldivar, R. J., Nokes, J., Steckel, G. L., Kim, H. I., & Morgan, B. A. (2010). The effect of atmospheric plasma treatment on the chemistry, morphology and resultant bonding behavior of a pan-based carbon fiber-reinforced epoxy composite. Journal of Composite Materials, 44(2), 137–156. https://doi.org/10.1177/0021998309345343

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.