Jonghwan Moon
Product group
Release & Process Aids

Putting the release agent on thicker is the usual response when concrete sticks to the forms and tears, but too heavy a film may fail to lower friction at the interface and can leave stains as well. What actually tears the surface can be missed coating, release agent washed off by rain or lost over time, a worn form face, a reactive agent given the wrong reaction time, or stripping too early, and sometimes two or more at once.

Background

The form will not come away from the concrete. Prised off with a bar, it brings a thin skin of the surface with it, leaving a roughly torn face with exposed aggregate behind, and corners break off. The torn face needs preparation and repair, and scraping off concrete stuck to the panel damages the form as well. Concrete durability depends in part on the quality of the cover zone, and the release method affects that quality through the surface finish (Shyha et al., 2016).

Two forces make concrete stick to formwork. One is mechanical keying, where cement paste works into the smallest asperities of the form face and becomes embedded, mainly on soft or irregular faces. The other is capillary force in very narrow water-filled gaps, which acts on hard, smooth faces, is large at the start of casting and falls slowly as the concrete hardens (Libessart et al., 2004). A release agent is the film that breaks both. There are barrier types, such as petroleum products, waxes and synthetic resins, that lay down a physical film, and reactive types whose ingredients, such as fatty acids, react with free lime in the concrete to form a metallic soap interface (NPCA, 2013).

So a torn surface means that at that spot the film failed to break the two forces, or the form came off before the concrete skin could withstand the bond. Where the tearing is, what it looks like and the history of that panel narrow this down considerably.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: mark the torn spots on the form panel layout, log when the release agent was applied and when the concrete was poured, the weather in between, when the forms were stripped and the concrete temperature up to then, and compare these with the release agent's technical data sheet, the TDS, and the stripping criteria in the specification.

Hypothesis 1: missed areas

If the tearing gathers in a few spots or bands, check whether those spots ever had release agent. Typical cases are places a spray struggles to reach, such as inside window box-outs, deep corners, around embedded items and at form joints; places where the agent was sprayed after the reinforcement went in so the bars blocked it; and panels cleaned or repaired without being recoated. Picture one case. The wall forms were stood and the reinforcement fixed before any release agent was sprayed, and on stripping, the skin had torn away at the inside corners of the window openings and along the lines where the bars ran.

Where there is no film, both forces act in full. Cement paste is made of very fine particles and is fluid early in casting, so it spreads over the form face and works into the smallest asperities, and adhesion is high (Libessart et al., 2004). In experiments where release agent was sprayed through the reinforcing mesh, it never reached the form face directly under the bars, and those spots wetted and hardened differently from their surroundings (Šliogeris et al., 2025). The American Concrete Institute specification requires form surfaces to be covered with a material that inhibits bond with concrete, and release agent to be applied according to the manufacturer's recommendations before reinforcement is placed (Malisch & Brown, 2017).

The clue lies in the shape of the tearing. See whether it coincides with lines spaced like the bars, with spots such as the inside of openings that a spray cannot angle into, or with the edges of repaired panels. Match the order of release agent application and reinforcement fixing in the work records, and before the next pour, shine a torch at a low angle before the forms are closed to look for breaks in the film's sheen, and wipe with a clean cloth to find spots where nothing comes off.

The answer lies in the order of work and in checking. Apply release agent to clean forms before the reinforcement goes in, and wipe off any that gets on the bars (NPCA, 2013). Coat corners and the insides of box-outs that a spray cannot reach separately by brush or cloth, keep a checklist recording who coated each panel and when, and recoat repaired or cleaned panels before assembly.

Hypothesis 2: agent lost before pour

If tearing comes from panels that were coated but waited a long time for the pour, suspect whether the film survived in between. That applies when coated forms stood outside for days, when it rained in the meantime, when steel forms heated up in midsummer sun, and when the pour slipped by a day or two. Suppose retaining wall forms were coated and stood on a Friday afternoon, it rained over the weekend, and the pour went ahead on Monday as planned. On stripping, the skin tears only on the upper and outer panels where rainwater ran down, while the side sheltered as if under eaves is fine.

Rain washes the film away. Precast industry guidance says forms stored outside, even briefly, should be walked past to make sure rain has not washed the release agent off, and that dust and debris should be kept off once forms are coated (NPCA, 2013). Heat thins the film. When the sun heats oiled moulds they can reach 40 to 60°C, and the release agent's viscosity drops as temperature rises (Libessart et al., 2004). A thinned film can run down vertical faces and leave the top thin. Where the film thins or breaks in this way, the paste bonds directly to the form face just as where there was no film at all.

Trace the records backwards. Find the gap between application and pour for each panel and the rain and temperatures in between, and lay them over the torn spots. Tearing that gathers on rained-on faces, sunlit faces or the upper parts of standing panels adds weight to this hypothesis. From the next pour, wipe each panel with a white cloth just before concreting to confirm the film is still there, and take the surface temperature of sunlit panels with an infrared thermometer.

If loss of film is the cause, move application closer to the pour. Cover coated forms against rain and dust, and check or recoat panels that were rained on or whose pour slipped, as the TDS specifies. In midsummer, coat and pour in the cooler hours, and if forms must stand outside for long, treat the coat that protects them from rust in storage separately from the coat applied for the pour.

Hypothesis 3: worn form face

If tearing keeps recurring on certain panels only, look at those panels' faces. Typical cases are plywood whose film has peeled to expose the grain, scratched and pitted steel panels, panels carrying hardened paste from the last pour, rusted panels, and spots that have been welded or patched. Sometimes, with the same release agent and the same mix, tearing starts on the same panels only after a certain number of reuses. Under raking light, the peeled patches on those panels have almost exactly the shape of the torn spots.

A damaged face increases keying and weakens the film. On steel form walls, roughness was Ra 0.3 µm on a new face but reached 1.6 µm on a worn one, and where hollows were up to 15 µm deep, the thin oil film could not fully do its lubricating job. The same study explains that on soft or irregular faces, mechanical keying dominates adhesion (Libessart et al., 2004). In comparisons of new and used panels, too, results depended on the roughness of the form face, and rougher panels soaked up more of the water-miscible agents (Savukaitis et al., 2021). What is soaked up leaves a thinner film on the face, and exposed grain and pits become places for the paste to key into.

The first thing to look at is how torn spots match panels. Group the tearing by panel number to see whether it gathers on certain panels, then examine those panels under raking light for peeled film, scratches, hardened residue and rust, and compare them with the torn shapes. Logging the number of uses per panel shows after how many the trouble begins, and putting a new panel in the same position for the next pour confirms it.

Once the panels are identified as the cause, repair them or take them out of service. After each pour, remove hardened residue without damaging the face, remove rust, and reseal or replace plywood whose film has peeled. Set a reuse limit for each panel type, and on absorbent faces adjust the application method as the TDS specifies.

Hypothesis 4: reaction time off

If tearing appears on new steel forms or forms that have stood idle while a reactive release agent is in use, look at reaction time. This happens when new forms arrive, their factory anti-rust coating is wiped off and release agent is sprayed for a pour that same day; when concrete goes in straight after coating without waiting the time the TDS sets; and when the reaction is slow on a cold day but the schedule runs as usual. New steel forms are an example. On their first use, release agent was sprayed and concrete placed straight away, and a thin skin tore away across the whole panel; after a few more uses of the same panels, the tearing gradually eased.

A reactive release agent reacts twice. First, its fatty acids react with the metal face to build a protective layer of metallic oleate, called seasoning, and only once this layer exists can fatty acid applied afterwards stay on the surface, rather than migrating into the metal, to react with free lime in the concrete. The same guidance says new forms should have their anti-rust coating removed and release agent applied liberally and left for at least four hours, preferably 24, and notes that forms in the sun season faster because of the higher temperature (NPCA, 2013). On the concrete side, esters meet calcium oxides and turn into insoluble carboxylates, that is soap, forming a film that keeps the concrete from sticking; in one study of this reaction, too much active matter disturbed the arrangement of the molecules and raised viscosity at the interface, so friction did not fall (Libessart et al., 2004). The amount of soap formed also depended on the fines and superplasticiser in the mix (Bouharoun et al., 2012).

Start by confirming which kind of agent is in use. Find in the TDS and the safety data sheet, the SDS, whether it is reactive and whether there is a waiting time and temperature condition between coating and pour, and match these against the actual work records. Note too whether the torn panels were new or long idle, whether they were seasoned, how many hours after coating the pour took place, and what the temperature was that day. Tearing on new panels that eases as reuses mount is a reasonable sign of incomplete seasoning.

If reaction time is the cause, season new forms before their first pour, and after coating wait the time the TDS sets before concreting. Allow extra time on cold days, and do not lay reactive agents on too thick. If a change of mix has shifted the amount of fines or superplasticiser substantially, check release on a small test panel first.

Hypothesis 5: stripped too early

If tearing appears widely regardless of panel, the surface skin peels thinly and corners break easily, look at stripping time. It can happen as the weather turns cold, when the usual stripping schedule is kept unchanged, when form turnaround is hurried, and with retarded mixes or thin members. Think of an early winter morning. The wall forms came off the morning after the pour as usual, the skin came away on the panels over wide areas, and the corners crumbled at the press of a hand.

Low temperature slows setting and strength gain. A rule of thumb holds that a drop of about 10°C in concrete temperature roughly doubles the setting time; forms are kept on for 1 to 7 days depending on the rate of strength gain, weather and loading, and field-cured cylinders or non-destructive methods are recommended to estimate in-place strength before stripping (NRMCA, 2014). United States occupational safety rules likewise forbid removing forms and shores until the employer determines that the concrete has gained enough strength to carry its own weight and the loads it will take, and require that determination to rest on conditions in the plans and specifications or on a standard test indicating compressive strength (OSHA, n.d.). At the interface, capillary force in water-filled gaps falls only slowly as the concrete hardens (Libessart et al., 2004), so early stripping pulls a still-weak skin with an adhesion that has not yet eased.

Start by measuring the concrete temperature. Gather concrete and air temperature records from pour to stripping, and compare the tearing with what happened when the same member was stripped on the same schedule on a warm day. Estimate the actual strength from field-cured cylinders or by the maturity method, which estimates strength from the temperature history (ASTM International, 2019). Tearing spread widely together with broken corners, concentrated on cold days, puts this hypothesis in front.

If the schedule is the cause, set stripping by strength rather than by date. Strip once the strength the specification requires has been confirmed by cylinders or maturity measurement, keep the concrete warm on cold days with insulating blankets or insulated forms, and reset the stripping schedule each season. If form turnaround must speed up, review with the mix designer ways to raise early strength in the mix.

Finding the cause

Before investigating each of the five hypotheses in turn, look at the records already on hand and at the torn spots. Coating order, dates of application and pour, weather, stripping date and concrete temperature are in the site diary and weather records, and panel numbers and torn spots can be overlaid on one layout drawing. Inspecting panels under raking light and reading the TDS do not take long either.

The pattern of the tearing separates the routes. Tearing gathered in a few places, such as lines along the bars or the insides of openings, points to missed coating; on rained-on faces or the upper parts of standing panels, to film lost before the pour. Tearing that recurs on the same panels points to the form face, and tearing concentrated on the first use of new or long-idle panels points to the reaction time of a reactive agent. A thin skin peeling widely regardless of panel, with crumbling corners and concentrated on cold days, points first to stripping time.

If that still does not settle it, change one thing at a time at the next pour: fit a new panel at the suspect position, move coating to just before the pour, season new panels in advance, or delay stripping until strength is confirmed. Keep everything else as it was apart from the one change, or there is no telling what worked, and photograph the torn area the same way as before the change for comparison.

The final check is whether the tearing has stopped, and what has become of the forms and the surface. Cast the same member a few more times to see that the tearing does not return, and if the fix involved more release agent, check that stains or bugholes have not increased. Precast industry guidance also notes that excessive release agent leads to staining (NPCA, 2013).

Several hypotheses can occur together on one wall. A worn panel soaks up release agent and thins the film, and if that panel is also rained on, the film disappears faster still. On cold days, the concrete's strength gain and the reactive agent's reaction slow together. In such cases, fix stripping time by strength first, then look at coating and panel condition. While stripping stays early, the skin keeps tearing whether panels or coating change, and there is no reading what has improved.

Limits and cautions

Required stripping strength and timing, release agent coverage and waiting time, and seasoning methods differ by member, mix, form material, release agent and climate, so numeric decisions follow the specification and the product's TDS. Timing for stripping structural members and removing shores is for the structural engineer to decide, and where repairing a torn face could affect cover or durability, agree the repair method with the designer first. Fatty acids in reactive agents also react with metals such as brass, bronze and aluminium, so check the materials of spray equipment and embedded items too (NPCA, 2013).

Safety matters too. Follow the product's SDS for protective equipment and ventilation with release agents, and avoid breathing in spray mist. Prising a stuck form off with a bar can make the panel drop or spring suddenly, so support its weight and keep people clear while working, and do not remove shores from members whose strength has not been confirmed (OSHA, n.d.). Release agent on decks and floors makes them slippery, so wipe it up at once.

Sources

  1. ASTM International. (2019). ASTM C1074-19e1, Standard practice for estimating concrete strength by the maturity method. https://doi.org/10.1520/C1074-19E01
  2. Bouharoun, S., Vanhove, Y., Djelal, C., De Caro, P., & Dubois, I. (2012). Interactions between superplasticizer and release agents at the concrete/formwork interface. Materials Sciences and Applications, 3(6), 384–389. https://doi.org/10.4236/msa.2012.36055
  3. Libessart, L., Djelal, C., De Caro, P., & Cavrot, J.-P. (2004). Physicochemical and tribological characterization of release agents. In Concrete structures: The challenge of creativity, fib Symposium, Avignon. https://www.afgc.asso.fr/app/uploads/2018/05/075-Djelal.pdf
  4. Malisch, W. R., & Brown, H. J. (2017). Examination and evaluation of ACI 347.3R-13 "Guide to formed concrete surfaces" [Final report]. ASCC Education, Research & Development Foundation, RMC Research & Education Foundation, ACI Foundation. https://ascconline.org/Portals/ASCC/ACI347_3R-13-Guide-Formedoncrete-Surfaces_5-4-2017.pdf
  5. National Precast Concrete Association [NPCA]. (2013). Tech notes: Proper application of release agents. https://precast.org/wp-content/uploads/101123_Resources_ProperApplicationofReleaseAgentsTechBrief.pdf
  6. National Ready Mixed Concrete Association [NRMCA]. (2014). CIP 27, Cold weather concreting. https://www.nrmca.org/wp-content/uploads/2021/01/27pr.pdf
  7. Occupational Safety and Health Administration [OSHA]. (n.d.). 1926.703, Requirements for cast-in-place concrete. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/laws-regs/regulations/standardnumber/1926/1926.703
  8. Savukaitis, G., Daukšys, M., Juočiūnas, S., Grinys, A., & Kriptavičius, D. (2021). The influence of new and used formwork coated with different release agents on the appearance of the formed concrete surface. Journal of Building Engineering, 42, 102807. https://doi.org/10.1016/j.jobe.2021.102807
  9. Shyha, I., Richardson, A., Coventry, K., & Ponton, H. (2016). Mould release technologies with regard to concrete surface finish. Magazine of Concrete Research, 68(2), 87–98. https://doi.org/10.1680/macr.15.00067
  10. Šliogeris, I., Rekus, D., Juočiūnas, S., Borg, R. P., & Daukšys, M. (2025). Investigating reinforcement shadow visibility on formed concrete surfaces using visual inspection and colour variation analysis. Buildings, 15(7), 1140. https://doi.org/10.3390/buildings15071140

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.