KALTECKOREA

BlogApplication notes

Why does rust converter not turn the rust black?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Remediation

Doubting the product or brushing on another coat is the usual response when rust converter does not turn black, but the black colour only forms when the chemical meets and reacts with iron in the rust, so unless the condition that kept them apart is found, the extra coat tends to stay unchanged too. What actually lies behind it can be too little rust to react, a surface blocked by oil or old paint, low temperature, a weak converter or too little reaction time, and sometimes two or more at once.

Background

Converter was brushed evenly over rusted pipe supports and steelwork joints, yet the next day the rust is still brown, or has turned black only in patches. Some areas carry a milky, cloudy film, and on others there is hardly a sign that anything was applied. The crew doubts the product or brushes on another coat, and the topcoat schedule slips accordingly.

Areas that stay brown may be areas where unconverted rust remains, and a coating laid over them can lift together with that rust. In a study comparing commercial converters, the reaction stayed mostly in the outer layer of the rust (Barrero et al., 2001), and a US military research evaluation found that converter performance depends more on the amount and type of rust, and on the permeability of the coating laid over it, than on chemical bonding to the rust (Emeric & Miller, 1993). Recoating again and again without knowing why costs product and labour, and often ends with the rust being stripped and the job started over.

The active ingredient in rust converter is usually tannin, phosphoric acid or a mix of the two. Tannin grips iron ions with neighbouring hydroxyl groups and forms ferric tannate, a dark blue-black compound that barely dissolves in water; the iron comes either from the rust or from steel dissolved by the acid in the liquid (Pardini et al., 2001). Oak tannin formed sparingly soluble complexes with ferric iron between pH 1 and 7, and on rusted steel mainly one type of complex formed (Gust & Suwalski, 1994). Rust components also react to different degrees: in infrared analysis lepidocrocite reacted most readily, while goethite and magnetite reacted less (Nasrazadani, 1997).

So the black colour is the product of the chemical meeting and reacting with iron in the rust. If the colour has not changed, there was little iron to meet, the two never met, or they met but reacted slowly. In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph the areas that turned black and those that did not, and record the surface before application, the air and steel temperatures that day, whether the liquid was diluted and how many hours after application it was checked, then compare these with the product's technical data sheet, the TDS.

Hypothesis 1: too little rust

It shows up when converter goes on new steel, on faces ground almost to bare metal, on faces with only a light bloom of rust, or on steel still carrying the blue-black mill scale formed in rolling. In the international rust grades, the first grade is a surface largely covered with adherent mill scale and with little if any rust (ISO, 2007). Picture the ends of recently delivered steel sections, brushed with converter because a little rust had appeared. A day later the surface is still its original blue-grey, and only the edges where rust had shown have darkened slightly.

The black film is built from iron in the rust, so little rust means little ferric tannate. In conservation guidance, each further coat of tannic acid brought the film closer to the desired thickness and colour, and heavy corrosion took longer to react and needed more coats than light rust or bare metal (CCI, 2013). A military evaluation tied converter performance to the amount and type of rust, and phosphoric acid tests found the degree of conversion varied strongly with how long the steel had rusted (Emeric & Miller, 1993; Almeida et al., 1997). On light rust the film forms correspondingly thin, and a thin film is pale, so the change hardly shows.

Mill scale is a different oxide from rust. It is the iron oxide layer formed when steel is rolled at high temperature, built up in layers of wüstite, magnetite and haematite (Chen & Yuen, 2003). Magnetite was among the rust components least reactive with tannin or phosphoric acid (Nasrazadani, 1997). Mill scale is also blue-black to begin with, so even if some reaction happens at the surface, the difference is hard to see by eye.

Look at photographs taken before application, if any exist. If not, find an untreated piece from the same lot and grade its rust against the standard's photographic references, deciding whether the surface is bright bare metal, blue-black mill scale or brown rust. Then see whether the areas that turned black match the areas that had rust. If only the rusted spots changed and the rest stayed as it was, the chemical did its work and there was simply no rust to change.

A surface with almost no rust is not a job for converter. Treat bare metal or tightly adhering mill scale with the surface preparation and primer suited to that surface, and use converter only on the rust condition the TDS specifies. On light rust that turned only faintly darker, apply one more coat if the TDS allows it, but do not build it up thick just to get the colour.

Hypothesis 2: blocked surface

It occurs on frames splashed with oil around machinery, on steel stored with rust-preventive oil, on handles carrying grease and hand grime, and on railings with patches of old paint. The same applies when old paint lingers thinly over the rust, or when the rust was wiped down with an oily rag. Converter goes onto a pump base just after maintenance. The liquid beads and runs off behind the brush, and the next day the bolt surrounds and lower edges are still brown, while only the upper face that oil never reached has turned black.

Whether it is tannin dissolved in water or a converter carried in a water-based resin dispersion, the reaction only happens once the liquid soaks into the rust and meets iron. On an oil film that repels water, the liquid cannot spread and beads instead; the standard test of splashing water on a cleaned surface to see whether the film of water breaks is a way of finding exactly this kind of hydrophobic film (ASTM International, 2021). Sound paint offers no iron to react with, and paint left thinly over rust blocks the liquid's path to it. Commercial converters did not penetrate deeply even into bare rust, and the reaction stayed in the outer layer (Barrero et al., 2001), so one more layer of oil or paint in front of the rust cuts the chance of contact further. That is why conservation guidance calls for dirt, oil and grease to be removed before tannic acid is applied (CCI, 2013).

Water gives the first answer. Sprinkle a little clean water on an area that did not change and see whether it spreads evenly or beads and breaks up, then wipe with a white cloth dampened with solvent to see whether oil comes away. Scrape old paint with a knife point to see whether a paint layer remains over the rust. If the brown areas match the oil splash side, the places hands touch or the patches of old paint, with sharp boundaries, this hypothesis is the likely one.

Remove oil and grease with solvent or a cleaner before applying converter. A solvent cleaning standard defines the condition of a surface from which visible oil, grease and contaminants have been removed, and this step comes before other surface preparation (SSPC, 2015). If a cleaner was used, rinse with water and let the surface dry before application. Scrape off loose old paint; where rust lies beneath paint, strip the paint to expose the rust first, and do not apply converter over old paint that is still sound.

Hypothesis 3: too cold

Outdoor work in winter, steel that cooled overnight in an unheated store, north faces that never see the sun and early-morning work all fall under this hypothesis. Heavy steel stays cold for a while even after the air has warmed. Say converter goes onto the supports of an outdoor pipe rack on an early winter morning, and someone returns around midday. The sunny side of the columns has begun to darken, but the shaded side is still brown as if wet, with milky, cloudy patches here and there.

Colour comes slowly on a cold surface because of reaction rate. Chemical reactions slow as temperature falls, so less ferric tannate forms in the same time, and conservation guidance has the tannic acid solution warmed to about 50 °C before it is brushed on (CCI, 2013). A converter containing a water-based resin dispersion faces a second threshold. For the resin particles to fuse into a film, the temperature must be at or above the minimum film formation temperature; below it, the particles dry as a loose packing that leaves a white, opaque, powdery film (Keddie, 1997). Cold steel also gathers dew easily. Under the international standard, condensation is considered likely unless the surface is more than 3 °C above the dew point, the temperature at which water vapour in the air condenses (ISO, 2017), and the condensed water dilutes the converter.

This hypothesis can be measured. Take the steel temperature with a contact surface thermometer, work out the dew point from air temperature and relative humidity, and look at the gap between them. Compare the readings with the TDS minimum application temperature, and see whether the brown areas cluster on shaded faces, faces near the ground or heavy members that warm slowly. If a milky film appeared, consider whether it marks resin that failed to form a film.

If the steel is colder than the TDS minimum or close to the dew point, postpone the work. Apply around midday when the sun has warmed the steel, leaving time for reaction and drying before sunset. Indoors, heat the steel first and keep the converter container somewhere warm until use. For a film that has already turned white and cloudy, follow the TDS on whether to wipe it off or recoat.

Hypothesis 4: weak converter

It happens when water is added to make a thick liquid spray better, when the converter is diluted to stretch it over a large area, or when an old container is not shaken and only the clear liquid at the top is used. The same thing happens when a brush worked over rust is dipped back into the original can all day long. A painter working across a large tank base notices in the afternoon that the liquid in the can has turned darker than it was in the morning. The faces done in the morning have turned black, while brown still shows through on the faces done in the afternoon.

Turning rust black takes enough tannin and acid to react with the iron in it. In conservation guidance, raising the tannic acid concentration from 2.5% to 5% gave a much darker, thicker film; the guidance adjusts the solution to pH 2.2 to 2.4 with phosphoric acid, and says to discard the solution and start again with fresh once it turns black in the container (CCI, 2013). Liquid that has turned black in the can has likely already reacted with iron carried in on the brush and used up part of its tannin.

The strength of the acid changes the result as well. The amount of iron tannin binds varied with tannin type and pH, and the degree to which phosphoric acid transforms rust depended strongly on acid concentration (Pardini et al., 2001; Almeida et al., 1997). In tests adding phosphoric acid to a tannic converter, pH and phosphate also governed adhesion between rusted steel and an epoxy coating (Li et al., 2021). Adding water dilutes tannin and acid together and raises the pH, so less black compound forms on the same rust and the colour stays pale.

Pour the leftover liquid and liquid from a new container side by side into clear cups to compare colour and consistency, and measure the pH of both with pH paper. If water was added, check how much against the dilution the TDS allows. Brush new and used liquid onto two separate patches of the same rusted plate, and the difference in colour a day later settles the question.

Dilute only when the TDS allows it, and only at the ratio it gives. Shake the container well before use, pour the working amount into a small pot, and never return leftovers to the original can. When the liquid in the pot darkens, discard it and pour fresh, and recoat faces left pale with fresh liquid as the TDS directs.

Hypothesis 5: too little time

This is the case when, on a tight maintenance schedule, the result is judged a few hours after application, when the topcoat follows straight away, or when rain or a hose wash arrives soon after application. Heavily rusted faces make it more likely. A stair railing treated in the morning is inspected after lunch: only the pits have turned black so far, and the broad faces are still brown. Pushed by the schedule, one section is topcoated in that state, and the next section is left until the following day.

The reaction between tannin and rust does not finish in one step. In conservation guidance the colour usually began to change quickly in pitted areas, but heavy corrosion took longer to react and needed more coats (CCI, 2013). The liquid's path into the rust is not short either: commercial converters did not reach the metal surface, and the reaction stayed mostly in the outer layer (Barrero et al., 2001). The film also needs time to settle. Paint drying has separate defined stages, set to touch, fully cured and ready to recoat (USACE, 1995), so a surface dry to the touch is not necessarily ready for the next step. If rain washes the surface before the reaction is complete, the liquid left to meet the rust is reduced.

Record the time of application, the time of inspection and the temperature in between, and compare them with the TDS reaction time and recoat interval. Photograph the same spot from the same angle a day later and compare whether the colour has deepened; that shows whether time was short. Where only the pits are black and the broad faces brown, also consider whether thick rust is still reacting.

Judge the result only after the time set in the TDS has passed. On thick rust, add coats as far as the TDS allows, each once the previous one has dried; conservation guidance likewise brushes off flaky film with a dry brush once a coat has dried and applies the next, repeating until the desired thickness and colour are reached (CCI, 2013). Postpone the work when rain is forecast, and apply the topcoat only once the converted layer meets the TDS recoat conditions.

Finding the cause

Most of the five hypotheses can be sorted out with a few photographs, the work record and the leftover liquid. Start with the surface and the liquid, which can be checked on the spot, and leave comparisons that need a day's wait until after.

The shape of the unchanged areas is the first clue. Patches with sharp edges around bolts, where hands touch or where old paint remains suggest oil or paint blocking the way; whole faces of bare metal or blue-black mill scale left unchanged suggest there was little rust to change in the first place. Areas clustered on shaded faces and heavy members, with a milky haze, point to low temperature, and colour that fades in the order the work was done points to diluted liquid or liquid already spent in the can. Black pits with brown broad faces may simply mean the reaction is still under way.

Next come the checks that take minutes: the water-break check, surface temperature against dew point, and the pH of the used liquid. If water beads on the surface, deal with the oil film first; if the steel is near the dew point or below the TDS minimum, deal with temperature; and if the used liquid has a higher pH than fresh liquid or has darkened, deal with the liquid.

If that still does not settle it, run a control trial. Mark out a few palm-sized patches on the same rusted member and change only one thing per patch: fresh against used liquid, degreased against not degreased, warm against cold. Looking at the colour after one day and after two also shows whether reaction time was short. Change several things at once, and there is no telling which one made the difference.

The hypotheses can overlap. On a cold morning, dew dilutes the liquid while the reaction slows, and liquid that beads on an oil film runs off before it has a chance to react. In such cases make the surface clean and warm, redo one area with fresh liquid, and if it still does not change, go back to the amount and type of rust and check whether that face is bare metal or mill scale. The last check is the colour just before topcoating: do not topcoat any area that has not turned black.

Limits and cautions

Dilution ratio, minimum application temperature, reaction time and recoat interval differ by product, so numeric decisions follow the product's TDS. Converter has been studied as an alternative to blasting, but the military evaluation records that earlier tests had found commercial converters to perform poorly and unreliably (Emeric & Miller, 1993). For rust on bridges, pressure equipment, structural members and other safety-related parts, do not judge by colour alone; get a coatings specialist and the asset owner to confirm.

Converters may contain acids such as phosphoric acid, so follow the product's safety data sheet, the SDS, for gloves, eye protection and ventilation. Rinse any splash on skin or eyes with water at once. When degreasing with solvent, keep ignition sources away and ventilate well, and collect oily rags in a lidded metal bin.

Sources

  1. Almeida, E., Pereira, D., Figueiredo, M. O., Lobo, V. M. M., & Morcillo, M. (1997). The influence of the interfacial conditions on rust conversion by phosphoric acid. Corrosion Science, 39(9), 1561–1570. https://doi.org/10.1016/S0010-938X(97)00058-9
  2. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  3. Barrero, C. A., Ocampo, L. M., & Arroyave, C. E. (2001). Possible improvements in the action of some rust converters. Corrosion Science, 43(6), 1003–1018. https://doi.org/10.1016/S0010-938X(00)00139-6
  4. Canadian Conservation Institute [CCI]. (2013). Tannic acid coating for rusted iron artifacts (CCI Notes 9/5). Government of Canada; first published 1989, revised 2013. Retrieved November 2026. https://www.canada.ca/en/conservation-institute/services/conservation-preservation-publications/canadian-conservation-institute-notes/tannic-acid-rusted-iron-artifacts.html
  5. Chen, R. Y., & Yuen, W. Y. D. (2003). Review of the high-temperature oxidation of iron and carbon steels in air or oxygen. Oxidation of Metals, 59(5–6), 433–468. https://doi.org/10.1023/A:1023685905159
  6. Emeric, D. A., & Miller, C. E. (1993). Rust transformation/rust compatible primers. In Technology 2002: The Third National Technology Transfer Conference and Exposition, Vol. 2. NASA. https://ntrs.nasa.gov/citations/19930012993
  7. Gust, J., & Suwalski, J. (1994). Use of Mössbauer spectroscopy to study reaction products of polyphenols and iron compounds. Corrosion, 50(5). https://doi.org/10.5006/1.3294344
  8. International Organization for Standardization [ISO]. (2007). ISO 8501-1:2007, Preparation of steel substrates before application of paints and related products: Visual assessment of surface cleanliness, Part 1: Rust grades and preparation grades of uncoated steel substrates and of steel substrates after overall removal of previous coatings. https://www.iso.org/standard/43426.html
  9. International Organization for Standardization [ISO]. (2017). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products: Tests for the assessment of surface cleanliness, Part 4: Guidance on the estimation of the probability of condensation prior to paint application. https://www.iso.org/standard/58061.html
  10. Keddie, J. L. (1997). Film formation of latex. Materials Science and Engineering: R: Reports, 21(3), 101–170. https://doi.org/10.1016/S0927-796X(97)00011-9
  11. Li, Y., Lei, B., & Guo, X. (2021). Influence of phosphoric acid on the adhesion strength between rusted steel and epoxy coating. Coatings, 11(2), 246. https://doi.org/10.3390/coatings11020246
  12. Nasrazadani, S. (1997). The application of infrared spectroscopy to a study of phosphoric and tannic acids interactions with magnetite (Fe3O4), goethite (α-FeOOH) and lepidocrocite (γ-FeOOH). Corrosion Science, 39(10–11), 1845–1859. https://doi.org/10.1016/S0010-938X(97)00060-7
  13. Pardini, O. R., Amalvy, J. I., Di Sarli, A. R., Romagnoli, R., & Vetere, V. F. (2001). Formulation and testing of a waterborne primer containing chestnut tannin. Journal of Coatings Technology, 73(913), 99–106.
  14. SSPC: The Society for Protective Coatings [SSPC]. (2015). SSPC-SP 1, Solvent cleaning.
  15. U.S. Army Corps of Engineers [USACE]. (1995). Painting: New construction and maintenance (EM 1110-2-3400). Department of the Army.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.