KALTECKOREA

BlogApplication notes

Why do copper tubes in cooling water systems pit through?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Heat Transfer & Cooling

Plugging the holed tube or fitting a new one is the usual response, but if the water and tube conditions that made the hole are unchanged, new tubes can pit through again. What actually lies behind it can be azole inhibitor spent by oxidising biocide, erosion-corrosion at high velocity, ammonia or sulphide contamination, carbon film or flux left from manufacture or installation, or soft water of low pH, and sometimes two or more at once.

Background

A chiller's condensing pressure starts to wander, or the cooling water side of a process heat exchanger smells of the process fluid. With the plant stopped and a tube pulled, the inner wall shows a pinhole, with green or white corrosion products clustered round it in small mounds. Copper pipework carrying the same cooling water begins to weep near its joints.

A single hole may be small, but the loss is not. Every plugged tube removes heat transfer area, and the remaining tubes must carry the same duty, so the cooling margin disappears. Refrigerant or process fluid leaking into the cooling water, or water leaking into the process, can turn into product contamination and environmental trouble, and in the end into a long stop to replace the whole tube bundle.

In water, copper protects itself with a thin film of copper oxide on its surface. While that film stays even, corrosion is very slow, but where it breaks at one spot, that small spot keeps dissolving inwards until the wall is perforated: pitting, a localised corrosion concentrated at points. How robust the film is depends heavily on water composition; higher alkalinity improved passivity and raised the potential at which pitting starts, while high ratios of certain other anions lowered it (Cong et al., 2009).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: cut out and keep a length of the holed tube, note whether the holes sit near the tube inlet or are scattered along it, and compare the records of cooling water pH, residual chlorine and azole level with the treatment chemical's technical data sheet, the TDS, and the control ranges in the treatment programme.

Hypothesis 1: spent azole

Systems open to air, such as cooling towers, take an oxidising biocide like chlorine or bromine to control microbes, and protect copper with an azole, an inhibitor made for copper. This hypothesis moves to the front when biocide is increased or shock-dosed repeatedly in the warm season when microbes grow, while the azole dose stays as usual. In midsummer, algae spread in a cooling tower and chlorine dosing was raised sharply for a while. When a heat exchanger is opened at service a few weeks later, the inside of the tubes is patched with dark and greenish stains instead of the usual even brown.

Azoles such as benzotriazole and tolyltriazole adsorb on copper and copper oxide and build a thin film of copper–azole complex that keeps oxygen and ions away from the metal (Finšgar & Milošev, 2010). The trouble is that this film and the azole in the water share the water with an oxidising biocide. In tests mimicking cooling water conditions, copper acted as a catalyst for free chlorine to break down tolyltriazole, and the same azole protected copper better alongside monochloramine than alongside free chlorine (Hsieh et al., 2010). Once the azole runs down, what is left is chlorine and bare copper. In tests under drinking water conditions, pits started sooner as free chlorine rose, and even moderate chlorine eventually produced severe pitting (Sarver & Edwards, 2012).

First measure whether azole actually remains in the water. Measuring at the supply and after the heat exchanger shows how much is lost within the circuit, and that figure is compared with the dose and with the target level in the treatment programme. For residual chlorine, pull from the records not just the average but the height and frequency of shock doses. If copper in the water and the weight loss of copper corrosion coupons moved together with the period of higher chlorine, the weight of evidence falls on this hypothesis.

With the cause narrowed to spent azole, change the way the two chemicals meet. Feed azole away from the biocide injection point, and raise the azole level around shock doses so the film holds. Bring residual chlorine back within the treatment programme's range, and where chlorine must stay high, review with the treatment supplier a disinfection approach less harsh on copper protection or an inhibitor that stands up better to chlorine.

Hypothesis 2: high velocity

If holes cluster just inside the tube inlets or where flow turns and strikes, at elbows and tees, suspect the flow itself. This happens after a pump is upsized, when several leaking tubes are plugged and the same flow is forced through fewer tubes, when debris lodged at the tube sheet inlet deflects a jet to one side, and when hot water circulates fast. In a plant that fitted a bigger cooling water pump during an expansion, the exchanger opened at the next year's service shows smooth grooves following the flow just inside the inlets of many tubes, with the rest of each tube sound.

Erosion-corrosion starts when flowing water strips away the protective film. Each copper alloy has a limit of wall shear stress, the force with which water scours the wall; above it, the corrosion product film is worn away and localised or accelerated general corrosion follows, and that limit differed widely between alloys (Efird, 1977). In tests on copper water tubing carrying continuously flowing aerated water at pH 8, the highest velocity without erosion-corrosion was 3 m/s at 65°C and 6 m/s at 30°C, lower at pH 6.5, and the authors advised a safety margin in practice because these were laboratory values (Knutsson et al., 1972). In the same study, larger tubes ran into trouble at lower velocities than small ones.

Checking starts with arithmetic. Dividing the cooling water flow by the number of open tubes and their internal cross-section gives the velocity in the tubes, and the figure rises as more tubes are plugged. Look for debris, shells and scale fragments lodged at the tube sheet inlets, and see whether holes and grooves are confined to a short length at the inlet or spread along the whole tube. Wall thickness changes over the full tube length can be mapped with eddy current examination for copper tubes (ASTM International, 2018b).

If velocity is the cause, bring the flow back within design first. Trim the pump flow or add a bypass, and where many tubes are plugged, consider bringing the bundle replacement forward. If inlet turbulence is the problem, discuss inlet protection inserts with the exchanger maker, and improve upstream strainers to keep debris out. Where high velocity cannot be avoided, consider changing to an alloy that tolerates a higher shear stress.

Hypothesis 3: ammonia or sulphide

The contaminants that are especially hard on copper are ammonia and sulphide. Ammonia gets in through leaks from ammonia refrigeration plant or process exchangers, or when treated sewage effluent still carrying ammonia is used as makeup. Sulphide comes from polluted raw water, water left to stagnate and turn foul, and sulphate-reducing bacteria growing under deposits. This happened at a food plant running ammonia refrigeration. After a small leak on the condenser side, the smell around the cooling tower changed, and a few months later fine cracks were found in brass tubes near the tube sheet.

Ammonia corrodes copper by forming soluble complex ions with it, yet in tests under cooling water conditions its corrosiveness became negligible when tolyltriazole was present (Hsieh et al., 2010). Put the other way, ammonia does its damage when azole is short. Some copper alloys carrying residual stress suffer stress corrosion cracking in ammonia, and a standard test method uses ammonia vapour to gauge how susceptible such alloys are (ASTM International, 2018a). Sulphide attacks by another route. In tests on seawater condenser alloys, sulphide pollution increased corrosion of copper alloy tubes and tube sheets and, depending on conditions, caused pitting, preferential attack at welds and dealloying, in which one alloy component leaches out, with a severity sensitive to water temperature (Gehring et al., 1983).

Measure ammonia and sulphide in the cooling water with field test kits or laboratory analysis. If ammonia shows up, pressure test the process exchangers and refrigeration plant one by one to find the leak, and compare with the level in the makeup water to tell whether it comes from inside the plant or from outside. For sulphide, take a rotten-egg smell, a black film inside the tubes and long-stagnant sections as clues. Look at the form of damage too: cracks near the tube sheet or at bends point more towards stress corrosion cracking, and welds or joints attacked first point more towards sulphide.

With a contaminant confirmed, stopping the leak comes first, and meanwhile keep azole at the upper end of the treatment programme's range. Where treated sewage effluent is used as makeup, review pretreatment to lower ammonia with the water treatment supplier. Remove dead legs or flush them regularly, and clear deposits to leave sulphate-reducing bacteria fewer places to grow. For an alloy that has cracked, agree stress relief or a change to an alloy less sensitive to ammonia with the exchanger maker.

Hypothesis 4: carbon film or flux

When holes start appearing in new tubes or pipework not long after installation, look at what the tube itself brought in rather than at the water. Typical cases are a thin carbon film left where drawing lubricant burned during annealing at the tube mill, flux that ran inside joints during soldering or brazing, and a system not flushed well enough before commissioning. A newly laid cooling water line starts to show pinholes within a few years, and the holes gather just downstream of joints, where flux would have run.

Carbon film is an old problem. Pitting of condenser tubes was investigated at power stations cooling their condensers with fresh water concentrated in cooling towers, and it was found to resemble the pitting of copper water pipes caused by carbon film formed during manufacture, although many tube makers disagreed (Retief, 1973). A recent study explained that on copper pipe covered with carbon residue, galvanic corrosion, crevice corrosion and oxygen concentration cells form along the edge of the film and cause localised attack, and benzotriazole eased this by forming its complex over the whole surface, film included (Lee et al., 2021). Flux is deliberately aggressive so as to clean the joint, so residue left behind is the problem. The standard for copper tube fluxes tests residue aggressiveness by the resistivity of its solution in water and requires the area where flux reacted to be clean, free of corrosion and residue (ASTM International, 2016).

The clues are where the holes are and what the bore surface looks like. Holes gathered downstream of joints point more towards flux, while holes scattered along the tube regardless of joints point more towards a manufacturing film. Split a holed tube lengthwise and look for a thin dark film on the bore or greenish residue caked round the joints, and if needed have a laboratory analyse the film for carbon and the residue for its make-up. Ask the installer for the pre-commissioning flushing records and the type and amount of flux used.

If film or residue looks to be the cause, removing it from the remaining pipe comes first. Flush flux out thoroughly, and agree a chemical clean suited to the material for carbon film with the tube maker or a specialist cleaning firm. After cleaning, build a protective azole film on the copper before returning to service. For future work, use flux that meets the standard and only as much as needed, make pre-commissioning flushing an acceptance item, and when buying new tubes, write a limit on carbon residue on the bore into the purchase specification.

Hypothesis 5: soft, acidic water

Soft water, low in calcium and bicarbonate, comes from using reverse osmosis permeate, condensate or rain-fed surface water as makeup, and pH drops when acid fed to prevent scale is overdosed. It can also fall sharply in a short time when a pH probe drifts or an acid pump fails to stop. One weekend, the probe in a pH control loop drifted and more acid than usual went in until it was put right on Monday. Over the following months, holes appear in tube after tube, and the cooling water copper record still shows a spike from that weekend.

Water on the acidic side dissolves the film that protects copper. The amount of copper released from new copper pipe was governed by the solubility of copper hydroxide, and under the same conditions raising pH reduced copper release (Edwards et al., 1996). For pitting, alkalinity also helps the film: higher alkalinity improved passivity and raised the potential at which pitting starts (Cong et al., 2009), so in soft, low-alkalinity water the film is that much weaker. Low pH also compounds flow effects; in the copper tube tests mentioned earlier, water at pH 6.5 caused erosion-corrosion at lower velocities than water at pH 8 (Knutsson et al., 1972).

Start by scanning the continuous pH record from end to end for short dips. Averages and daily manual readings do not reveal them. Measure alkalinity and hardness of makeup and circulating water to confirm whether the water is soft, and check that the acid pump run log and acid consumption agree with the pH record. If copper in the cooling water rose together with the dips in pH, this hypothesis firms up.

The core remedy is pH control. Calibrate the pH probe at fixed intervals, interlock the acid pump to stop on a low-pH alarm, and cap how much acid the feed system can deliver at once. For circuits on soft makeup, reset the alkalinity and pH control ranges with the treatment supplier and hold azole within range under them. For tubes already thinned, use eddy current results on remaining wall to set the order of replacement.

Finding the cause

There is no need to investigate all five at once. pH, residual chlorine, azole level and ammonia either have records already or can be measured on the spot, so they can be looked at without a shutdown. Pulling and splitting tubes, eddy current examination and analysis of films and residues need a stop, so they come after.

Where the holes are is the biggest clue. Holes confined to a short length at the tube inlet or where flow turns lead first to velocity; holes gathered downstream of joints, to flux; holes scattered along new tubes, to a manufacturing film. Cracks near the tube sheet or at bends lean towards ammonia stress corrosion cracking, while welds and joints attacked first, together with a black film, lean towards sulphide. Broad thinning across many tubes along with holes sends the search to water pH and azole.

Timing comes next. After an increase in biocide dosing, put spent azole first; after a pump change or many plugged tubes, velocity; after a process leak or a long shutdown, ammonia and sulphide; soon after installation, carbon film and flux; after a fault in the pH loop, low pH.

If that still does not settle it, bleed a little water through a side-stream test loop fitted with copper corrosion coupons or short tube sections, and change one condition at a time. Move the azole feed point, lower residual chlorine or reduce velocity, then compare coupon weight loss and cooling water copper on the same basis as before the change. The job can be called done only when eddy current examination at set intervals shows wall loss has stopped growing (ASTM International, 2018b).

The hypotheses often appear together. When chlorine strips the azole, ammonia regains its corrosiveness in the gap (Hsieh et al., 2010), and low pH pulls down the velocity at which erosion-corrosion begins (Knutsson et al., 1972). Since localised attack on carbon-filmed tube eased when azole was sufficient (Lee et al., 2021), a film combined with a shortage of azole can make holes sooner. In such cases, put the water chemistry right first, pH, azole and residual chlorine, then look again at velocity and the tube itself, because while the water is unsettled, the effect of changing the hardware cannot be compared fairly.

Limits and cautions

Suitable azole level, residual chlorine, pH, alkalinity and allowable velocity differ by alloy, whether copper, brass or copper-nickel, and by water quality and treatment approach, so numeric decisions follow the treatment chemical's TDS and programme and the exchanger maker's guidance. In an exchanger with toxic or flammable process fluid on the other side of the tubes, one hole is a safety issue, so do not keep running on floor judgement alone, and leave eddy current interpretation and metallographic analysis to specialist bodies.

Safety matters too. Chlorine does harm when inhaled or in contact with skin and eyes (NIOSH, n.d.), so handle biocides and acids with the protective equipment and ventilation their safety data sheets, the SDS, require, and store and feed hypochlorite and acid separately so they never mix. Before opening an exchanger, isolate both fluids, release pressure and let it cool, and lock out before work begins.

Sources

  1. ASTM International. (2016). ASTM B813-16, Standard specification for liquid and paste fluxes for soldering of copper and copper alloy tube. https://doi.org/10.1520/B0813-16
  2. ASTM International. (2018a). ASTM B858-06(2018), Standard test method for ammonia vapor test for determining susceptibility to stress corrosion cracking in copper alloys. https://store.astm.org/b0858-06r18.html
  3. ASTM International. (2018b). ASTM E243-18, Standard practice for electromagnetic (eddy current) examination of copper and copper-alloy tubes. https://store.astm.org/e0243-18.html
  4. Cong, H., Michels, H. T., & Scully, J. R. (2009). Passivity and pit stability behavior of copper as a function of selected water chemistry variables. Journal of The Electrochemical Society, 156(1), C16. https://doi.org/10.1149/1.2999351
  5. Edwards, M., Schock, M. R., & Meyer, T. E. (1996). Alkalinity, pH, and copper corrosion by-product release. Journal AWWA, 88(3), 81–94. https://doi.org/10.1002/j.1551-8833.1996.tb06521.x
  6. Efird, K. D. (1977). Effect of fluid dynamics on the corrosion of copper-base alloys in sea water. Corrosion, 33(1), 3–8. https://doi.org/10.5006/0010-9312-33.1.3
  7. Finšgar, M., & Milošev, I. (2010). Inhibition of copper corrosion by 1,2,3-benzotriazole: A review. Corrosion Science, 52(9), 2737–2749. https://doi.org/10.1016/j.corsci.2010.05.002
  8. Gehring, G. A., Foster, R. L., & Syrett, B. C. (1983). Effect of sulfide on the corrosion and protection of seawater-cooled condenser alloys. In CORROSION/83. NACE. https://doi.org/10.5006/C1983-83076
  9. Hsieh, M.-K., Dzombak, D. A., & Vidic, R. D. (2010). Effect of tolyltriazole on the corrosion protection of copper against ammonia and disinfectants in cooling systems. Industrial & Engineering Chemistry Research, 49(16), 7313–7322. https://doi.org/10.1021/ie100384d
  10. Knutsson, L., Mattsson, E., & Ramberg, B.-E. (1972). Erosion corrosion in copper water tubing. British Corrosion Journal, 7(5), 208–211. https://doi.org/10.1179/000705972798322856
  11. Lee, Y.-H., Hong, M.-S., Ko, S.-J., & Kim, J.-G. (2021). Effect of benzotriazole on the localized corrosion of copper covered with carbonaceous residue. Materials, 14(11), 2722. https://doi.org/10.3390/ma14112722
  12. National Institute for Occupational Safety and Health [NIOSH]. (n.d.). Chlorine. NIOSH Pocket Guide to Chemical Hazards. Retrieved November 2026. https://www.cdc.gov/niosh/npg/npgd0115.html
  13. Retief, R. (1973). Corrosion of condenser tubes due to carbonaceous film on the surface. British Corrosion Journal, 8(6), 264–269. https://doi.org/10.1179/000705973798321847
  14. Sarver, E., & Edwards, M. (2012). Inhibition of copper pitting corrosion in aggressive potable waters. International Journal of Corrosion, 2012, 857823. https://doi.org/10.1155/2012/857823

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.