KALTECKOREA

BlogApplication notes

Why do deep-drawn parts split at the corners?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Lowering the blank holder force is the usual first response to deep-drawn parts splitting at the corners, but if something else raised the wall tension, lowering the force tends to trade the split for wrinkles. What actually lies behind it can be a thin or uneven lubricant film, a blank holder force that is off, die radius or surface, a shift in sheet properties, or too little viscosity or extreme pressure additive, and sometimes two or more at once.

Background

The press is drawing square cups or box-shaped parts with rounded corners, and the wall just above the bottom corner, or the wall at the corner, comes out split. Once splitting starts it often repeats at the same spot, and split parts cannot be repaired, so they go straight to scrap. Small cracks that are hard to see are worse. Missed at inspection, they can come back from the customer as leaks or fractures after welding, painting and assembly.

In deep drawing, the blank holder presses on the edge of the sheet, the flange, while the punch pushes the sheet into the die opening to form a wall. The force to pull the flange towards the die, friction at the holder and die faces, and the force to bend and unbend the sheet over the die radius all pass through the wall to the punch, so when that tension exceeds the strength of the thinnest point, the wall splits, usually near the punch radius (Marciniak et al., 2002). In a square part, the flange at the corners is squeezed hard in the circumferential direction and resists being drawn in, so deformation concentrates in the corner wall. A study of square cups by simulation and experiment likewise found the greatest thinning at the cup corner, explained by excessive stretching there (Younis et al., 2018).

So a corner splits in one of two ways: the tension in the wall rises, or the sheet carrying it thins further or could bear less to begin with. Lubrication, holder force, tooling, the sheet and the lubricant's additives all feed into one of these two, so where and when the split appears narrows the cause sharply.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the split parts, mark where and in which direction each split runs, log the coil number, lubricant amount, blank holder force and running time when splitting began, and compare them with the lubricant's technical data sheet, the TDS, and the tool settings.

Hypothesis 1: thin or uneven film

A lubricant film causes trouble not only when there is too little but also when it is uneven. It happens when a clogged roller or spray nozzle leaves one side of the blank or the corner areas short, when oil drains down a stack of blanks so the top and bottom sheets differ, after the amount is cut to save cost, and on the first run when a rested tool is dry. Monday morning, and the press starts again after a weekend off. Split corners turn up among the first parts, and then, an hour or so later, the same settings produce only good parts.

Friction at the flange and the die radius adds directly to the force needed to draw the flange in. An analysis of lubrication in cup drawing found that the larger the calculated oil film thickness relative to the surface roughness of the sheet, the smaller the metal-to-metal contact and the lower the friction, and that lubrication on the die face and the die radius changed markedly during forming (Mizuno & Kataoka, 1980). In flat strip drawing tests, the more viscous oil lowered friction more, and the effect of lubrication also depended on contact pressure (Szewczyk et al., 2022). On a production progressive tool, the first run after a rest started with relatively dry tooling and the local lubricant layer built up over time (Aha et al., 2021). Where the film is thin or missing, friction rises, wall tension rises with it, and the thinnest corner wall splits first.

Start by measuring how much is on the blank. Cut set areas from the corner zone and the centre of the same blank and weigh them before and after degreasing to get the amount by location, then compare it with the amount recommended in the TDS. Check nozzles and rollers for clogging and wear, and compare top and bottom sheets of a stack the same way. On formed parts, measure how far the flange was drawn in at each corner. Deep drawing tests that compare lubricants use this draw-in length, together with the highest blank holder force a cup survives without fracture, to rank lubrication performance (Kim et al., 2009).

If the coating was uneven, fix the applicator first. Clean clogged nozzles and replace worn rollers, then set the pattern so enough lubricant reaches the corner zones of the flange. Before the first run after a rest, pre-apply lubricant to the die radius and holder face, and do not leave blanks stacked for long. If the amount had been cut, bring it back into the TDS range, and if cutting again, do it one step at a time while counting splits.

Hypothesis 2: blank holder force off

The blank holder force is the lever that controls wrinkles and splits together, so turning it to fix one tends to bring out the other. Look at this hypothesis after cushion pressure was raised to remove flange wrinkles, when a sheet of different thickness came in but the force stayed the same, and when uneven cushion pin lengths or a worn holder face concentrate pressure at the corners. Take a day when an operator saw fine wrinkles at the flange edge and raised cushion pressure a step. The wrinkles went, and that afternoon corner splits began.

The harder the holder presses, the greater the friction between flange and tooling, so drawing the flange in takes more force, and that force arrives as wall tension. Too little force, on the other hand, and the flange cannot resist circumferential compression and wrinkles. A review of research on blank holder force concluded that varying the force over the stroke, and from place to place on the blank, can widen the working window between splitting and wrinkling (Obermeyer & Majlessi, 1998). In cup drawing experiments and simulations, raising the holder force likewise reduced wrinkling but caused splits near the punch corners (Ahmed et al., 2026). In experiments on stainless steel square cups, excessive force kept the blank from flowing into the die and tore the upper corners, and raising force and blank size together produced tears running parallel to the bottom (Ünal & Özkan, 2025).

Begin by matching the force settings in the records against when splitting started. Measuring cushion pin lengths and checking the holder face for wear shows whether pressure is applied evenly. The shape of the remaining flange on formed parts is a clue too: if only the split corner was drawn in less, pressure or friction may have concentrated there. Time permitting, run trial draws at several force steps to find the force at which wrinkles first disappear and the force at which splits first appear, and see where the current setting sits between them.

If force is the cause, move the setting to the middle of those two forces, and adjust cushion pins and spacers so pressure does not concentrate at the corners. If the cushion can vary force over the stroke, consider separate forces for the early and late parts of the draw. Keep a value for each sheet in the setting table so the force is reset whenever thickness or grade changes. If wrinkles and splits appear on the same part, force alone leaves no window, so look at lubrication and tooling as well.

Hypothesis 3: die radius or surface

Suspect this hypothesis in tools designed with small die or punch corner radii, in tools whose radii changed after regrinding or weld repair, and in tools with scratches or metal stuck on the die radius. It applies all the more to sheets that tend to stick to tooling, such as stainless steel. Galling, where sheet material sticks to the tool face, and wear are typical friction problems in forming stainless steel sheet (Takaki et al., 2018). Turn a split part over and the scene is plain: vertical score lines run along the wall where it passed the die radius, and a fingertip run over the die corner radius catches on rough spots.

The sheet bends once as it goes round the die radius and straightens again as it enters the wall; the smaller the radius, the more force and friction this bending and unbending takes, raising wall tension, and a small punch radius concentrates that tension in a narrow zone (Marciniak et al., 2002). A study combining experiment and simulation found that smaller die radii increased both thinning and thickening in the wall (Ahmed et al., 2026). A bigger radius is not always the answer: in experiments on stainless steel square cups, enlarging the radius to 8 mm reduced wrinkling but caused localised stress build-up (Ünal & Özkan, 2025). Surface condition needs checking alongside the radius. Metal stuck on the die radius roughens the face and raises friction for every sheet that passes, and that friction adds straight onto wall tension.

Measure the die and punch corner radii with radius gauges or a replica and compare them with the drawing, marking any corners with a repair history. Search the die radius face for scratches and stuck metal under a magnifier, and check whether score lines on the part wall line up with the split corner. Measuring wall thickness at the corners and on the straight sides with a micrometer shows in numbers which corner has thinned unusually.

With the cause narrowed to tooling, restore the surface first. Remove stuck metal from the die radius and polish it back to its original finish, and for sheets where the problem keeps returning, review surface treatment or coating of the tool with the toolmaker. Changing a radius can trade one defect for wrinkles or another, so do it only after confirming with the tool designer through simulation or trial draws.

Hypothesis 4: sheet property shift

If, with tooling, lubricant and force unchanged, splitting began after a change of coil, supplier or grade, look at the sheet. Even within one specification, thickness and properties can vary from coil to coil inside tolerance, and a change of material batch is counted among the causes of an unstable production process (Aha et al., 2021). Picture the first day on a new coil. A part that had run well now splits at the same two of its four corners every time, and going back to leftover blanks from the previous coil brings good parts again.

How well a sheet withstands deep drawing depends heavily not on strength but on how well it resists thinning through its thickness. This property is expressed as the plastic strain ratio, the r value, the ratio of width strain to thickness strain in a tensile test, and the higher the r value, the less the sheet thins and the higher its limiting drawing ratio (Hosford & Duncan, 1999). The r value is measured separately in each direction, such as 0, 45 and 90 degrees to rolling, and the test method for sheet intended for deep drawing is set out in a standard (ASTM International, 2024). When r differs by direction, some places round the part thin less and others more, so with the same tool only the corners in a particular direction may split. In a cup drawing study, too, the r value by rolling direction strongly influenced thinning (Ahmed et al., 2026).

Lay the mill certificates of the new and previous coils side by side and compare yield strength, tensile strength, elongation, r value and thickness. If the certificate gives no r value, have a laboratory cut specimens from both coils and measure r in each direction, and measure thickness yourself at several points on the blank. Mark as well whether the splitting corners always sit at the same angle to the blank's rolling direction.

If results split by coil, set that coil aside and hand samples to the supplier along with the test certificate. Put a minimum r value and a thickness tolerance for this part into the purchase specification, and check them against the certificate for every incoming coil. Cutting blanks with a consistent rolling direction puts the directional differences in the same place every time, which also makes them easier to handle on the tooling side.

Hypothesis 5: low viscosity or EP

Look at the lubricant's viscosity and additives on afternoons when continuous running heats the tool, in hot weather, after a switch to a lower-viscosity lubricant, and after a product with chlorinated extreme pressure additive was replaced by another. Extreme pressure, or EP, additives react with the metal surface at contacts where pressure and heat are high, forming a film that keeps metal from welding to metal. A tool that ran without trouble in the morning grows too hot to touch by the afternoon, and from about then corner splits and score lines on the wall increase together.

Sheet forming done at room temperature actually gets quite hot. A study modelling the room-temperature forming of high-strength sheet predicted temperatures of up to 108 °C in the sheet and 181 °C in the tool, and validated this experimentally (Pereira & Rolfe, 2014). Lubricant viscosity falls as temperature rises; in tests friction increased as viscosity dropped, and early in a run friction conditions were unsettled by heat from plastic and frictional work and the drop in viscosity (Aha et al., 2021). Once the oil film thins and metal begins to touch metal, the remaining line of defence is the reaction film from the EP additive. In ironing stainless steel, a chlorinated additive reacted evenly with iron, chromium and nickel and gave a clearly stronger EP effect than a sulfur additive, which hardly reacted with chromium (Petrushina et al., 2000). Without enough of this film, the sheet sticks to the tool at high-pressure spots such as the corners, friction soars and the wall splits.

Measure tool temperature at the die radius and holder face with an infrared thermometer over running time, and log it alongside the split count. If splits rise with tool temperature, this hypothesis gains weight. Check the viscosity and EP content of the lubricant in use against its TDS, and match the date of any product change against when splitting began. If score lines on the wall and stuck metal on the die radius grew at the same time, suspect even more strongly that the film is failing.

If a heating tool is where it starts, look first at cooling and press speed. If the lubricant does not suit that temperature and pressure, choose with the supplier a product that holds its viscosity at high temperature, or EP additives suited to the sheet and the severity of the draw. Chlorinated paraffins have been used for forming sheets prone to galling, but efforts continue to replace them with less harmful lubricants for environmental and health reasons (Bay et al., 2010). A chlorine-free oil that combined a sulfur additive with calcium and zinc components completed a long run of stainless steel ironing without galling (Takaki et al., 2018). Chlorine-free options exist, then, but confirm any replacement product with trial draws on the actual tool before switching.

Finding the cause

There is no need to test all five hypotheses at once from the start. Clear them away beginning with the easiest to check. The amount of lubricant on the blank, cushion pressure records and tool temperature can be checked without a long stop, and coil numbers and mill certificates are already on file. Measuring radii and inspecting tool faces means taking the tool out, so it comes next.

When the splits appear is the first clue. Splits that cluster on the first run after a rest and then fade point to the lubricant film; splits that grow with running time point to tool temperature and the lubricant's viscosity and EP additives; splits from the day the force was changed point to holder force; and splits from a coil change point to the sheet. If, regardless of timing, they always come at the same corner, suspect that corner's die radius and surface, or the sheet's properties in that direction.

The look of the split part sorts causes too. Vertical score lines on the wall point first to rising friction, meaning the tool surface or the EP additives. If only the flange at the split corner was drawn in less, look at pressure or lubrication there; if the flange edge shows wrinkles as well as a split corner, force alone cannot fix it, so look at lubrication and die radius. If wall thickness measurements show that the unsplit corners have thinned too, the next split is close.

If the cause still will not separate, run control trials changing only one thing at a time. With blanks from the same coil, raise only the lubricant amount, lower only the force by one step, feed only blanks from the previous coil, and draw once with a cool tool and once with a hot one. Change several things together and there is no way to tell which one worked. Afterwards, compare splits per set output and corner wall thickness on the same basis as before the change; the job is done only when both figures have recovered.

Several hypotheses may be at work at once. Where the film is thin, sheet material sticks to the tool face more easily; the stuck face raises friction and heat; and on a hot tool viscosity drops and the film thins further. A sheet with a low r value narrows the working window under the same force and lubrication. In such cases, stabilise lubrication and tool temperature first, then revisit force, die radius and the sheet, because while friction and heat are unsettled, the effect of changing force or sheet cannot be compared fairly.

Limits and cautions

Suitable blank holder force, die radius, lubricant amount, and lubricant viscosity and EP additives differ by sheet, thickness, part shape and press, so numeric decisions follow the lubricant's TDS and the guidance of the tool designer and the sheet supplier. Measuring r values and judging forming limits are work for the laboratory and the tool designer, and for parts where a leak or fracture is a safety issue, such as pressure vessels or fuel system parts, do not release on the floor judgement that splits have stopped; have the quality engineer confirm with wall thickness checks and crack inspection.

Safety matters too. For lubricants and cleaners, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and limit exposure to metalworking fluids such as forming oils, which can harm health through skin contact and through breathing in mist (OSHA, n.d.). Inspect die radii and faces or reload blanks only after the press is fully stopped and locked out, and wear gloves against the sharp edges of split parts.

Sources

  1. Aha, B., Hettich, D., Veldhuis, M., & Filzek, J. (2021). Higher productivity in forming high-alloyed steel by temperature insensitive friction behavior. ESAFORM 2021: 24th International Conference on Material Forming. https://doi.org/10.25518/esaform21.2075
  2. Ahmed, R. R., Kara, İ. H., & Jweeg, M. J. (2026). Experimental and numerical investigation of thinning behavior in deep drawing of AISI 1008, CuZn30, and aluminum 1100. Materials Science, 32(3). https://doi.org/10.5755/j02.ms.43434
  3. ASTM International. (2024). ASTM E517-24, Standard test method for plastic strain ratio r for sheet metal. https://store.astm.org/e0517-24.html
  4. Bay, N., Azushima, A., Groche, P., Ishibashi, I., Merklein, M., Morishita, M., Nakamura, T., Schmid, S., & Yoshida, M. (2010). Environmentally benign tribo-systems for metal forming. CIRP Annals, 59(2), 760–780. https://doi.org/10.1016/j.cirp.2010.05.007
  5. Hosford, W. F., & Duncan, J. L. (1999). Sheet metal forming: A review. JOM, 51(11), 39–44. https://doi.org/10.1007/s11837-999-0221-5
  6. Kim, H., Altan, T., & Yan, Q. (2009). Evaluation of stamping lubricants in forming advanced high strength steels (AHSS) using deep drawing and ironing tests. Journal of Materials Processing Technology, 209(8), 4122–4133. https://doi.org/10.1016/j.jmatprotec.2008.10.007
  7. Marciniak, Z., Duncan, J. L., & Hu, S. J. (2002). Mechanics of sheet metal forming (2nd ed.). Butterworth-Heinemann.
  8. Mizuno, T., & Kataoka, H. (1980). A study of the lubrication mechanisms in deep drawing. Bulletin of JSME, 23(180), 1016–1023. https://doi.org/10.1299/jsme1958.23.1016
  9. Obermeyer, E., & Majlessi, S. (1998). A review of recent advances in the application of blank-holder force towards improving the forming limits of sheet metal parts. Journal of Materials Processing Technology, 75(1–3), 222–234.
  10. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids
  11. Pereira, M. P., & Rolfe, B. F. (2014). Temperature conditions during 'cold' sheet metal stamping. Journal of Materials Processing Technology, 214(8), 1749–1758. https://doi.org/10.1016/j.jmatprotec.2014.03.020
  12. Petrushina, I. M., Christensen, E., Bergqvist, R. S., Møller, P. B., Bjerrum, N. J., Høj, J., Kann, G., & Chorkendorff, I. (2000). On the chemical nature of boundary lubrication of stainless steel by chlorine- and sulfur-containing EP-additives. Wear, 246(1–2), 98–105. https://doi.org/10.1016/S0043-1648(00)00503-2
  13. Szewczyk, M., Szwajka, K., & Trzepieciński, T. (2022). Frictional characteristics of deep-drawing quality steel sheets in the flat die strip drawing test. Materials, 15(15), 5236. https://doi.org/10.3390/ma15155236
  14. Takaki, T., Kitamura, K., & Shibata, J. (2018). Development of chloride-free oil with sulfur-based EP additive for cold forming of stainless steel. Mechanical Engineering Journal, 5(2), 17-00449. https://doi.org/10.1299/mej.17-00449
  15. Ünal, E., & Özkan, U. (2025). AISI 304 östenitik paslanmaz çelik kare kapların derin çekme performansı: Kalıp geometrisi ve parametre optimizasyonu. Fırat Üniversitesi Mühendislik Bilimleri Dergisi, 37(2), 533–541. In Turkish with English abstract. https://doi.org/10.35234/fumbd.1699070
  16. Younis, K. M., Jabber, A. S., & Abdulrazaq, M. M. (2018). Experimental evaluation and finite element simulation to produce square cup by deep drawing process. Al-Khawarizmi Engineering Journal, 14(1). https://doi.org/10.22153/kej.2018.10.002

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.