Adding more defoamer is the usual response when foam will not break, but a defoamer works when its type and the way it goes in are right rather than through quantity, and too much leaves film defects such as craters. What actually lies behind the foam can be air drawn in during mixing and additions, a defoamer of the wrong type or compatibility, the wrong dosing point, high viscosity or a heavy surfactant load, and sometimes two or more at once.

Background

Long after the disperser has stopped, a white layer of foam still sits on top of the tank. Skim it off and measure the density, and it comes out below the formulated value; fill cans and the foam keeps them from taking their full measure. Panels painted from this batch show pinholes and small crater-shaped defects, and in an adhesive, bubbles trapped inside the applied layer reduce the bonded area.

Foam eats time. Batches occupy tanks longer while the foam dies down, filling slows, and product that overflows with the foam is lost. Bubbles left in the film spoil gloss and appearance, and pinholes leave holes in a film meant to keep out corrosion. Fine bubbles can even change how the coating flows during application (Reader et al., 2013).

In clean water, air bubbles quickly merge, rise and burst. Waterborne products contain surfactants, such as emulsifiers that stabilise the latex, wetting agents that lower water's high surface tension so it wets substrate and pigment, and dispersants that keep pigment evenly spread, and these gather on bubble surfaces, form a film and stabilise foam (Reinhardt et al., 1998). Surfactants slow the drainage of liquid from the bubble wall and also stop bubbles merging (Reader et al., 2013). A defoamer is a substance that enters this film and spreads across it to tear it apart, usually made of oils insoluble in water and hydrophobic particles (Karakashev & Grozdanova, 2012).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: take the order and timing of raw material additions, mixing speed and time, and batch temperature from the foaming batch's work order, and compare them with the dosing stage and conditions recommended in the technical data sheets, the TDS, of the defoamer and binder.

Hypothesis 1: air entrainment

A lot of air goes in when the high-speed disperser blade turns close to the liquid surface, when the tank holds little liquid as at the start of a batch, and when an unbaffled tank develops a vortex that hollows out the centre. Liquid dropped in from the top of the tank, or air leaking in at a pump suction, does the same. Consider a batch where the disperser was run at top speed to break in pigment quickly. The surface over the blade is hollowed out deeply, the tip of the vortex touches the blade, and a white thread of air is pulled down into the liquid at that spot.

The route by which mixing puts air in starts at the free surface. In an unbaffled stirred tank, the swirl from the blade forms a vortex at the centre, and once the vortex deepens enough to reach the blade, it sucks air into the liquid (Paul et al., 2004). A study that filmed bubbles drawn in from the free surface of an unbaffled tank at high speed reports that as the gap between surface and blade shrinks, surface instability takes over air entrainment, that blade speed strongly affects the size of the entrained bubbles, and that turbulent energy in the tank breaks them into smaller ones (Sung & Park, 2024). It is these finely broken bubbles that cause trouble. A small bubble rises at a speed proportional to the square of its radius and inversely proportional to the liquid's viscosity, so the smaller it gets, the far longer it takes to reach the surface (Pugh, 2016).

Look down into the tank while it mixes. Check whether the vortex reaches the blade, how deep the liquid is over the blade, and whether liquid entering the tank throws up spray. Take a sample at each stage and measure density with a density cup, then compare it with the calculated air-free density; the numbers show at which stage the air went in. If there is a circulation pump, check the suction-side joints for the sound of air being drawn in or streams of bubbles.

If air comes in from mixing, the fix lies with the equipment. Start high-speed dispersion only once the blade is well submerged, and reduce speed from the let-down stage, once pigment dispersion is complete. For tanks where the vortex reaches the blade, review baffles or an off-centre shaft with the equipment supplier, and feed liquid raw materials below the surface or let them run down the wall. Seal air leaks at the pump suction by tightening the joints.

Hypothesis 2: mismatched defoamer

Look at this hypothesis when the binder was changed to another grade but the defoamer was not, when the defoamer was switched to another type to save cost, or when a defoamer that worked well in a matt product was carried straight over to a high-gloss one. Drums of defoamer left standing so long that the contents settle or separate belong here too. On the floor, people say the defoamer dose was doubled, the foam stayed and the only result was craters in the film.

A defoamer has to get into the foam film before it can work. Its oil droplets enter the boundary between liquid and air and either spread over it or build a bridge across both faces of the film, and the film tears as that bridge becomes unstable. Droplets must clear a threshold to enter the boundary, and when that threshold is high, foam lingers even with defoamer present (Denkov, 2004). Particles such as hydrophobic silica mixed into the oil lower the threshold and strengthen the defoamer's ability to pierce the film (Garrett, 2016). That is why a coatings defoamer must be somewhat incompatible, meaning it does not mix in too readily, so that it moves to the boundary and does its job. Push that too far, though, and it causes film defects such as fish-eyes, craters and crawling, and mineral oil defoamers suit matt to medium-gloss acrylic and styrene acrylic products but can dull gloss definition in high-gloss ones (Reinhardt et al., 1998).

Laboratory comparison separates them quickly. Add the same amount of each candidate defoamer to the same base formula, entrain air under the same mixing conditions, and measure density, foam height and the time for foam to collapse. Draw each sample down on glass or test charts at the same thickness and look at craters and gloss together. For the plant's defoamer drum, sampling from top and bottom and checking that appearance and viscosity match shows whether it has separated.

If the defoamer is judged a mismatch, choose the type again rather than raising the dose. If the binder or gloss grade has changed, select a defoamer for that combination with the supplier, and test foam removal and film defects together under the same shear conditions as production. Use defoamer within its set shelf period, and mix the drum evenly before use.

Hypothesis 3: wrong dosing point

When the defoamer goes in is set by a single line in the work order, yet changing that line can change the outcome sharply. It matters when, for convenience, all the defoamer goes into the mill base with the pigment from the start, when it goes in before bead milling, and when the addition at the final adjustment stage is forgotten. Suppose that, to shorten the procedure, the whole defoamer charge was moved to the mill base stage; batches may then follow that are fine right after dispersion but foam up again during let-down and filling.

The size of defoamer droplets is set by the intensity and duration of the shear they meet on addition, and the harder the shear, the finer the droplets. Under violent dispersion such as bead milling, droplets break up very finely; adding an emulsion defoamer to the grind can shrink them so far that defoaming power drops sharply, and droplets below 1 µm across have repeatedly been found to have hardly any defoaming effect. The same study notes that many defoamers work well right after production but lose efficiency in storage (Reinhardt et al., 1998). Defoamers also wear out with use. A mixed oil and silica antifoam took longer and longer to break foam as foaming and collapse were repeated, which was explained by the oil being emulsified and used up (Pugh, 2016). Among foam control agents, the name defoamer usually goes to those that break existing foam quickly, but many combine fast action with lasting effect, and their speed depends on the setting they work in (Denkov et al., 2014). If the defoamer added at the start is broken up finely and worn out during a long dispersion, little is left to work at the later stages where foam actually forms.

Start by recording at which stage foam forms. Measure foam height and density at the mill base, right after dispersion, at let-down, at viscosity adjustment and at filling, and match them against when and how much defoamer went into that batch. Making the same formula in the lab two or three ways, changing only the defoamer dosing point, gives a good indication of whether timing is the cause. Also stir finished product again after a few days' storage to see whether foam returns.

If timing was the problem, the basic step is to go back to the stage the TDS recommends. Add emulsion defoamers away from the intense dispersion stage, and if foam must be controlled during dispersion, review with the supplier a separate defoamer suited to that stage. Where the formula calls for split addition, write the amount for each stage into the work order and add a check box so the final-stage addition is never missed.

Hypothesis 4: high viscosity

Foam lingers in high-viscosity adhesives, waterborne paints thickened with thickener, high-solids formulas, and batches made from raw materials brought in from a cold warehouse in winter. All the more so when the batch was stirred hard right after thickener went in. Follow one waterborne adhesive batch. After thickener went in and the batch was stirred for a long time to hit viscosity, the large bubbles on top have gone, but the whole liquid looks cloudy and stays that way even after a night in the can.

The cloudiness is fine bubbles dispersed through the liquid. Breaking large bubbles stabilised at the surface and releasing small bubbles and microfoam trapped in the liquid or beneath the film are two separate problems. Bubbles rise faster the larger they are, the greater their density difference from the liquid and the lower the viscosity, so the higher the viscosity and the thicker the film, the harder it is for small bubbles to reach the surface. A film's viscosity rises further as it dries, so bubbles that have not risen and burst before then stay behind as microfoam or leave pinholes (Reader et al., 2013). In latex products, small particles can produce high viscosity and form layers within the foam film that help foam last longer (Pugh, 2016).

Measuring viscosity and density together brings this side out. Record viscosity and batch temperature at the moment foam formed, keep a sample in a clear bottle, and watch over time whether bubbles rise and how far density recovers. If bubbles clear quickly when the same sample's viscosity alone is lowered by thinning or warming, viscosity is the cause. Also check in the records when thickener went in and how fast the batch was stirred afterwards.

If viscosity is the cause, change the order so that air removal is finished while viscosity is still low. Add thickener as late as possible and at low speed, and avoid high-speed mixing afterwards. In winter, keep raw material and batch temperatures within the TDS range so viscosity does not climb too far. For high-viscosity products where fine bubbles still remain, review vacuum deaeration equipment, or deaerators aimed at fine bubbles in the bulk, with the supplier.

Hypothesis 5: heavy surfactant load

This hypothesis comes forward when wetting agent or dispersant was added to fix another problem, when the latex was switched to a grade with more emulsifier, or when several additives each brought a little surface-active content and the total grew large. Suspect it if foam increased from the point a raw material changed, and the bubbles are large and firm and do not collapse even when stirred by hand. Foam complaints may begin the week after wetting agent was raised to solve a substrate wetting complaint.

Surfactants are the framework of a foam film. When the film thins, the surfactant layer lined up on the bubble surface draws liquid back through differences in surface tension, healing the film, and it slows liquid draining out of the film (Pugh, 1996). Waterborne coating formulas holding plenty of latex particles and a high surfactant concentration produce foam that many defoamers struggle to break. Above the critical micelle concentration, where micelles begin to form, surfactant molecules adsorb on hydrophobic particles and turn them hydrophilic, so particle-type defoamers may work poorly, and oil-based defoamers are used instead. The height of the threshold a defoamer droplet must clear to enter the boundary also varied widely with the combination of surfactant and defoamer (Pugh, 2016). The more surfactant there is, the stronger the opponent the defoamer has to beat.

Add up the surfactants in the formula raw material by raw material. Check the TDS and SDS of the binder, dispersant, wetting agent, thickener, biocide and other raw materials for surface-active content, and mark which ones and which amounts changed recently. Make samples step by step, binder alone, binder with wetting agent, then the full formula, shake or stir them under the same conditions, and compare foam height and collapse time; this shows which raw material builds the foam.

If surfactant proves excessive, first bring added wetting agent and dispersant back to what is needed, and work with the supplier to cover the remaining performance with grades that foam less. If the latex grade was changed, choose the defoamer type again to suit that grade. Whenever surfactant is added to fix another problem, include a foam test in the same approval step.

Finding the cause

A good order keeps the investigation short. Looking down into the tank, matching the work order against actual addition records, and measuring density and viscosity at each stage can all be done on the next batch. Lab comparisons that swap defoamers or surfactants come after that, and changes to equipment wait until the cause is confirmed.

The shape of the foam is a major clue. A thick, firm layer of large bubbles that lasts on the surface points to a heavy surfactant load or a mismatched defoamer, while a calm surface over a cloudy, low-density liquid means fine bubbles cannot escape, pointing to air entrainment from mixing and high viscosity. If foam is absent right after dispersion but appears at let-down or filling, look first at the dosing point; if it began when a raw material changed, look at the surfactant that material brought or how it suits the defoamer.

Read the film defects as well. More craters and fish-eyes suggest a defoamer that is too incompatible or too much of it, while more pinholes suggest fine bubbles that could not escape before the film dried. If one batch shows both heavy foam and craters, check the records for whether extra defoamer was added to suppress the foam.

If that still does not settle it, run control trials that change one thing at a time. Make the same formula with only the mixing speed lowered, only the defoamer type changed, only the dosing point moved, only the thickener delayed, or only the wetting agent reduced, and measure density, foam height, collapse time and film defects the same way for all. Change one thing at a time to know which one worked; the job is done only when density returns close to the calculated value and film defects do not rise.

The hypotheses tangle easily. High-speed mixing not only puts in plenty of air but also breaks defoamer droplets finely and weakens them, and once thickener is in, that air is locked in by high viscosity. A surfactant-rich formula turns the same air into firmer foam. In such cases, first put right the way air gets in, meaning mixing conditions and the order of additions, and then adjust defoamer type and amount again, because while air keeps coming in, any defoamer comparison gives unsteady results.

Limits and cautions

Defoamer type and amount, dosing stage, mixing speed and a suitable viscosity differ by binder, pigment and end use, so numeric decisions follow each raw material's TDS and the equipment supplier's guidance. The shear a defoamer meets in a small lab batch differs from that in a production tank, so results may not carry over directly; confirm any changed condition again at production scale. For regulated uses, such as food packaging adhesives or products that touch skin, check compliance with the relevant rules before introducing a new raw material.

Safety matters too. For defoamers, surfactants and thickeners, follow each product's safety data sheet, the SDS, for protective equipment and ventilation. Look into high-speed dispersers and bead mills, or take samples from them, only after the blade and shaft have fully stopped and the power is locked out, and keep vacuum deaeration equipment within the pressure limits in its manual. Overflowing product and foam make floors slippery, so clean them up at once, and treat wash water and waste liquid in line with local rules.

Sources

  1. Denkov, N. D. (2004). Mechanisms of foam destruction by oil-based antifoams. Langmuir, 20(22), 9463–9505. https://doi.org/10.1021/la049676o
  2. Denkov, N. D., Marinova, K. G., & Tcholakova, S. S. (2014). Mechanistic understanding of the modes of action of foam control agents. Advances in Colloid and Interface Science, 206, 57–67. https://doi.org/10.1016/j.cis.2013.08.004
  3. Garrett, P. R. (2016). The science of defoaming: Theory, experiment and applications. CRC Press. https://doi.org/10.1201/b15158
  4. Karakashev, S. I., & Grozdanova, M. V. (2012). Foams and antifoams. Advances in Colloid and Interface Science, 176–177, 1–17. https://doi.org/10.1016/j.cis.2012.04.001
  5. Paul, E. L., Atiemo-Obeng, V. A., & Kresta, S. M. (Eds.). (2004). Handbook of industrial mixing: Science and practice. Wiley-Interscience. https://doi.org/10.1002/0471451452
  6. Pugh, R. J. (1996). Foaming, foam films, antifoaming and defoaming. Advances in Colloid and Interface Science, 64, 67–142. https://doi.org/10.1016/0001-8686(95)00280-4
  7. Pugh, R. J. (2016). Bubble and foam chemistry. Cambridge University Press. https://doi.org/10.1017/CBO9781316106938
  8. Reader, C. J., Hegedus, C., Lai, K. T. G., Louis, C., el Ajaji, S., & Chaigneau, W. (2013, January). Novel zero-VOC deaerators for waterborne coatings. CoatingsTech, 22–28. https://www.paint.org/wp-content/uploads/2021/09/Zero-VOC-Deaerators-Waterborne-Coatings_Jan-2013.pdf
  9. Reinhardt, R. A., Heilen, W., Walhorn, E., Silber, S., & Adams, J. W. (1998). Defoamer selection in waterborne coatings. Journal of Coatings Technology, 70(885), 157–160. https://doi.org/10.1007/BF02730086
  10. Sung, H., & Park, H. (2024). Free-surface air entrainment into bubbles by a Rushton-type impeller in unbaffled stirred tank. Physics of Fluids, 36(6), 063335. https://doi.org/10.1063/5.0209873

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.