KALTECKOREA

BlogApplication notes

Why does descaling not restore heat exchanger performance?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Cleaning & Surface Prep

Running the descaler again is the usual response when a heat exchanger loses performance, but a descaler only dissolves acid-soluble scale on the surfaces it reaches, so repeating the same clean may not bring performance back. What actually lies behind it can be silica or calcium sulphate scale that acid will not dissolve, dead zones the circulation never reaches, too little temperature and time, spent acid, or an oil film left in place, and sometimes two or more at once.

Background

At a scheduled shutdown a descaler is circulated through a heat exchanger and the unit goes back on line, yet the outlet temperature still falls short of design and the pressure drop on the cooling water side has barely changed from before the clean. Stopping again for a second clean repeats the downtime, chemicals and waste disposal, while running on at reduced performance can mean burning more fuel and power to move the same heat, or slowing production. Heat exchanger fouling has long been treated as a problem that ends up in energy, production and maintenance costs (Müller-Steinhagen et al., 2011).

Scale is a layer formed when salts dissolved in water harden on a hot heat transfer surface. Its most common constituents are calcium carbonate and calcium sulphate, and how much of each builds up depends on flow velocity, heat flux, surface temperature and the concentration of the water (Helalizadeh et al., 2000). The acid at the heart of a descaler reacts readily with carbonates such as calcium carbonate and dissolves them, but not every scale dissolves in acid. That is why the choice of cleaning solvent is meant to rest on laboratory analysis of a deposit sample taken from the tubes or plates (Veolia, n.d.).

Performance that does not return means something is still on the heat transfer surface. What remains may be a component acid cannot dissolve, or oil that covered the surface before the acid could reach it; or it may be soluble scale that the solution never reached, that was circulated too cold for too short a time, or that outlasted acid already used up.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: gather inlet and outlet temperatures, flows and pressure drops from before and after the clean, together with the chemical, concentration, temperature, time and circulation flow used, compare them with the product's technical data sheet, the TDS, and if the exchanger can be opened, keep any deposit left behind.

Hypothesis 1: acid-insoluble scale

Where the raw water is groundwater or surface water high in silica, where a cooling tower concentrates the water over several cycles, or where the water is high in sulphate or has its pH trimmed with sulphuric acid, scales other than calcium carbonate can grow alongside it. They tend to bond hardest in evaporators, heaters and the plates at the hot inlet, where surface temperatures run high. Picture a plate heat exchanger opened after a clean. Most plates show bare metal, but a few on the side where hot water enters still carry a thin white film, smooth as glass.

Acid dissolves calcium carbonate because the carbonate meets the acid and turns into a soluble salt and carbon dioxide; calcium sulphate and silica have no such route. Calcium sulphate dissolves poorly in hydrochloric acid, so methods have been studied that convert it to calcium carbonate with a converting agent such as potassium carbonate while a chelating agent in the same solution dissolves it (Murtaza et al., 2022). Silica builds up on equipment as silicic acid dissolved in the water links up of its own accord into colloidal silica and silicate polymers (Ning, 2010).

A study of silicate scale reports that removing these deposits has relied on fluorine-based acids such as hydrofluoric acid, ammonium bifluoride and fluoroboric acid, that chelating agents combined with caustic dissolved a range of silicates, and that varied scale composition makes multistage cleaning necessary. The same study points out that silicate minerals conduct heat far worse than other deposits, which is why a thin residual layer alone, after most of the deposit is gone, can keep performance from returning (McCartney et al., 2017).

Scrape off a little of the remaining film and add a drop of dilute acid. If it fizzes and dissolves, it is carbonate; if it sits there without bubbling, it may be something other than carbonate, such as sulphate or silicate. Confirm the composition by sending a sample to a laboratory for crystal structure and elemental analysis, and look at the silica, sulphate and calcium levels and the cycles of concentration of the make-up and circulating water from the same period.

If the analysis finds sulphate or silicate, running the same acid for longer will not solve it. Take the results to the chemical supplier or a specialist cleaning contractor to plan a staged clean with a converting agent, chelating agent or fluoride-based chemical suited to the composition, and confirm compatibility with the materials. Afterwards, reset the concentration limits for silica and sulphate on the water treatment side so the same scale does not grow back.

Hypothesis 2: poor circulation

Look at this hypothesis when a small portable cleaning pump serves a large exchanger, in plate heat exchangers with narrow channels between plates, in shell-and-tube shells with spots flow barely reaches, such as behind baffles or at the edge of the tube sheet, and in piping layouts where air collects at the top. Flow also tends to be uneven when the solution runs in one direction only, or when several units are cleaned in series at once. The scene for this hypothesis: a cleaning pump is hosed onto the bottom drain of the exchanger, and when it is opened afterwards the lower plates are clean while scale remains in bands only in the upper corners and along the edge opposite the inlet.

The reaction between acid and scale happens only where acid reaches the surface, and acid near the surface is quickly diluted as it reacts. In a study measuring how fast hydrochloric acid dissolves calcite, the crystal form of calcium carbonate, the rate at room temperature was set not by the surface reaction but by how fast acid travelled to the surface, even at high rotation speeds (Lund et al., 1975). Where flow is weak, less fresh acid arrives, so less dissolves in the same time. Flow strength also varies widely within a single unit. In food equipment cleaning research, the shear stress acting on the wall varied greatly from spot to spot within a component, and how well each spot cleaned depended on that stress and on the nature of recirculation zones where flow turns and lingers (Jensen et al., 2005). Where air is trapped, the solution never touches the surface at all.

Start with circulation flow and pressure in the cleaning record. Check whether the cleaning rig's flow was far below the unit's normal operating flow, and whether there was barely any pressure difference across the unit during the clean. See whether air was vented from the top as the unit was filled. If the exchanger can be opened, sketch where scale remains and see whether it clusters where flow is weak: the top, the corners, the far side from the inlet. If chips from those spots dissolve readily in the same solution in the laboratory, the problem is flow rather than composition.

If flow is the cause, change the cleaning method. Use a circulation pump sized to the unit and its normal flow, fill from the bottom up and vent air at the top. Reversing the flow direction at intervals during the clean reduces dead zones that form on one side only, and when several units are linked, clean them one at a time. With plate units, pulling the remaining plates and soaking them separately is another option.

Hypothesis 3: too cold, too short

This hypothesis fits when solution from an outdoor tank is used unheated during a winter shutdown, when the solution is drained earlier than planned to keep to a tight schedule, or when thick scale built up over a long time gets the same time as a thin layer would. Say that on a midwinter maintenance day the solution in a cleaning tank standing outside was circulated without heating, and although foam was still rising in the tank, it was drained and the rinse begun because the next job was waiting.

The outcome of a clean is not set by the chemical alone. Cleaning research treats the result as set jointly, for a given deposit and cleaning fluid, by the chemical action, temperature, time and the mechanical action of flow, so that a shortfall in one has to be made up by another (Fryer & Asteriadou, 2009). The U.S. Department of Defense criteria for industrial water treatment have inhibited dilute acid preheated for boiler acid cleaning and kept at that temperature, and for circulation cleaning of smaller equipment such as heat exchangers, circulation continued until the reaction is complete, as shown by foam subsiding or the acid being used up (DoD, 2005). A cold solution reacts slowly, and cutting the time on top of that leaves behind scale that could have dissolved. Yet temperature cannot simply be raised at will. The corrosion inhibitors that protect steel in acid struggle to stay effective at high temperatures, which is why separate high-temperature formulations have been developed (Finšgar & Jackson, 2014).

Check the solution temperature in the record both at the tank and in the return from the exchanger. The tank may be warm while the solution cools along a long hose and through a cold unit. Look as well at the circulation time, how the foaming changed over it, and whether the acid strength in the return was still falling at the end. If strength was still dropping and foam still forming at the last reading, the clean stopped before the reaction finished.

For the next clean, heat the solution within the temperature range in the product's TDS and control it on the return temperature, and end the clean on the signs that the reaction is complete rather than on a time fixed in advance. Those signs are foam subsiding, acid strength in the return no longer falling, and dissolved calcium and iron levelling off. If the shutdown schedule is fixed, build in enough time for those signs from the start.

Hypothesis 4: spent acid

Acid can run out partway when thick scale meets a batch of solution made up only to the unit's volume, when old carbon steel equipment carrying much rust and iron oxide is cleaned, or when the clean is run by the clock without measuring strength. Think of a day when two exchangers on the same line were cleaned one after the other from a single tank of solution. The first one recovered, but the second, which received the same solution next, is almost as it was before the clean.

Acid is consumed in proportion to the scale it dissolves. Each molecule of calcium carbonate dissolved takes two molecules of hydrogen chloride and leaves calcium chloride, water and carbon dioxide behind. Rust and iron oxide use up the same acid. So the Department of Defense criteria for industrial water call for measuring and recording acid strength at least every hour during the clean, and for adding or replacing solution once strength falls below 3%, since most of its dissolving power is then spent (DoD, 2005). Another guide has circulation cleaning continue until the chemical concentration and the dissolved iron and copper reach a constant value (Veolia, n.d.). Once the acid is used up, the solution may keep circulating while the remaining scale stays put.

Draw samples of the returning solution at regular intervals during the clean, titrate the acid strength and compare it with the starting value. If little strength is left, the acid ran short. Without records, estimate from the pH or acid strength of the solution just before draining. Next time, estimate the amount to be dissolved from scale thickness and area, and allow more for equipment carrying much rust and iron oxide.

If depletion was the cause, write the solution volume and top-up rules into the cleaning procedure. When strength falls below a set value, top it up or change to fresh solution, and do not clean several units in succession from one tank. Since a build-up of dissolved iron can mean more attack on steel surfaces, set an upper limit for iron content together with the chemical supplier as well.

Hypothesis 5: oil left on scale

When a heat exchanger with oil on one side, such as a compressor cooler or a hydraulic or lube oil cooler, develops a small leak in a tube or plate, when process oil gets into the cooling water, or when the process side itself is being cleaned, an oil film may cover the scale. An air compressor aftercooler is cleaned and opened, and the remaining scale has a glossy brown sheen, with rinse water beading on it instead of spreading evenly.

Acid dissolved in water cannot wet oil. When scale is covered by an oil film, the acid cannot reach the scale beneath, and scale bound up with oil dissolves only at the surface and then stops. That is why boiler and heat exchanger cleaning guidance removes oil and grease first by hot alkaline cleaning, and where oil is present, puts the alkaline clean ahead of the acid clean so the oil does not interfere (Veolia, n.d.). The standard practice for cleaning and descaling stainless steel likewise sets a precleaning step that removes oil and grease before scale is stripped with acid (ASTM International, 2017).

Pour clean water over the surface. If the water breaks up and beads instead of spreading as an even thin film, there is oil on the surface. Wipe it with a white cloth to see whether oil comes off. In the laboratory, the share of organic matter in a deposit chip can be measured by how much weight it loses when soaked in solvent and when burned. If oil is confirmed, trace where it came from, starting with pressure on the oil side and any oil floating on the cooling water.

Scale mixed with oil calls for a different order. Remove the oil first with an alkaline degreaser or a solvent, rinse, confirm that water spreads evenly over the surface, and only then move on to the acid clean. Rinse thoroughly between stages so that degreaser and acid do not mix. If a leak is behind it, find and seal the leaking tube or plate rather than repeating the clean, or the same contamination will build up again.

Finding the cause

Five hypotheses do not mean five separate investigations from the outset. Start with the records already on hand. Flow, temperature, time and the change in acid strength during the clean are on record, so circulation, temperature and time, and spent acid can largely be settled without opening the unit again. The composition of what remains and any oil need a sample, so they come next.

Next is how the scale remained. If it is left in bands in only some places, such as the upper corners or far from the inlet, look first at circulation dead zones; if it has thinned evenly over the whole surface but is still there, look first at too little temperature and time or at spent acid. A hard, smooth film at the hot inlet that does not fizz in acid points to acid-insoluble scale, and a glossy surface on which water beads points to an oil film.

If that still does not settle it, run a beaker test. Soak a chip of the remaining deposit in the same solution at the same strength, at a temperature within the TDS range. If it dissolves readily in the beaker, composition is not the issue, and the flow, temperature, time and amount of acid on site need another look. If it does not dissolve even in the beaker, move on to composition analysis; if a chip degreased first then starts to dissolve, an oil film was in the way.

Confirm the outcome by performance. Compare before and after at the same flow and inlet temperature and see whether the overall heat transfer coefficient, outlet temperature or pressure drop has returned to the clean-condition value. If operating conditions differ too much for a direct comparison, find records from the same season and load and compare against those. The clean is finished only when the numbers have recovered.

The hypotheses can overlap. A silica layer may lie beneath carbonate scale covered in oil, and thick scale both spends the acid quickly and blocks weak-flow spots further. In such cases, remove the oil first, dissolve the carbonate with acid while holding strength and temperature, then analyse whatever is still left and add a stage suited to it. While the earlier stages are unsettled, there is no telling whether the remaining deposit is truly insoluble.

Limits and cautions

Acid type and strength, temperature, time, corrosion inhibitor and material compatibility differ by chemical and equipment, so numeric decisions follow the chemical's TDS and the heat exchanger maker's guidance. Gaskets in plate heat exchangers, stainless steel, copper alloys and aluminium can be damaged depending on the chemical, so check before use. Plan staged cleans for sulphate and silicate scale, and any clean using fluoride-based chemicals, with a specialist cleaning contractor or the chemical supplier.

Safety matters too. For acids and degreasers, follow the product's safety data sheet, the SDS, for protective equipment and ventilation. Acid cleaning releases gases such as carbon dioxide and hydrogen, so ventilate enclosed spaces and keep flames away; the Department of Defense criteria require the equipment used to be explosion-proof and acid-resistant (DoD, 2005). Take particular care with hydrofluoric acid and fluoride-based chemicals. Dilute hydrofluoric acid can cause almost no pain on contact and then serious injury 12 to 24 hours later, and fluoride taken into the body can alter blood levels of calcium, magnesium and potassium (ATSDR, n.d.). Dispose of spent solution, with the metals dissolved in it, according to the applicable regulations.

Sources

  1. Agency for Toxic Substances and Disease Registry [ATSDR]. (n.d.). Medical management guidelines for hydrogen fluoride. Centers for Disease Control and Prevention. Retrieved November 2026. https://wwwn.cdc.gov/TSP/MMG/MMGDetails.aspx?mmgid=1142&toxid=250
  2. ASTM International. (2017). ASTM A380/A380M-17, Standard practice for cleaning, descaling, and passivation of stainless steel parts, equipment, and systems. https://store.astm.org/a0380_a0380m-17.html
  3. Finšgar, M., & Jackson, J. (2014). Application of corrosion inhibitors for steels in acidic media for the oil and gas industry: A review. Corrosion Science, 86, 17–41. https://doi.org/10.1016/j.corsci.2014.04.044
  4. Fryer, P. J., & Asteriadou, K. (2009). A prototype cleaning map: A classification of industrial cleaning processes. Trends in Food Science & Technology, 20(6–7), 255–262. https://doi.org/10.1016/j.tifs.2009.03.005
  5. Helalizadeh, A., Müller-Steinhagen, H., & Jamialahmadi, M. (2000). Mixed salt crystallisation fouling. Chemical Engineering and Processing: Process Intensification, 39(1), 29–43. https://doi.org/10.1016/S0255-2701(99)00073-2
  6. Jensen, B. B. B., Friis, A., Bénézech, T., Legentilhomme, P., & Lelièvre, C. (2005). Local wall shear stress variations predicted by computational fluid dynamics for hygienic design. Food and Bioproducts Processing, 83(1), 53–60. https://doi.org/10.1205/fbp.04021
  7. Lund, K., Fogler, H. S., McCune, C. C., & Ault, J. W. (1975). Acidization—II. The dissolution of calcite in hydrochloric acid. Chemical Engineering Science, 30(8), 825–835. https://doi.org/10.1016/0009-2509(75)80047-9
  8. McCartney, T. R., Gharaibeh, S., & Shank, R. (2017). Improved methods for removal of silicate deposits. Proceedings of International Conference on Heat Exchanger Fouling and Cleaning – 2017. https://heatexchanger-fouling.com/wp-content/uploads/2021/09/32_McCartney_Improved-Methods-for-Removal-of-Silicate.pdf
  9. Müller-Steinhagen, H., Malayeri, M. R., & Watkinson, A. P. (2011). Heat exchanger fouling: Mitigation and cleaning strategies. Heat Transfer Engineering, 32(3–4), 189–196. https://doi.org/10.1080/01457632.2010.503108
  10. Murtaza, M., Alarifi, S. A., Rasm, M. Y., Kamal, M. S., Mahmoud, M., & Al-Ajmi, M. (2022). Single step calcium sulfate scale removal at high temperature using tetrapotassium ethylenediaminetetraacetate with potassium carbonate. Scientific Reports, 12, 10085. https://doi.org/10.1038/s41598-022-14385-6
  11. Ning, R. Y. (2010). Reactive silica in natural waters — A review. Desalination and Water Treatment, 21(1–3), 79–86. https://doi.org/10.5004/dwt.2010.1229
  12. U.S. Department of Defense [DoD]. (2005). Unified facilities criteria UFC 3-240-13FN: Industrial water treatment operation and maintenance. https://www.wbdg.org/FFC/DOD/UFC/ARCHIVES/ufc_3_240_13fn_2005.pdf
  13. Veolia Water Technologies & Solutions [Veolia]. (n.d.). Chapter 15: Chemical cleaning of steam generator systems. In Handbook of industrial water treatment. Retrieved November 2026. https://www.watertechnologies.com/handbook/chapter-15-chemical-cleaning-steam-generator-systems

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.