KALTECKOREA

BlogApplication notes

Why does release agent build up on die-casting dies?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Release & Process Aids

Cleaning the die more often is the usual response to release agent build-up, but if the conditions that built the layer stay the same, the same layer grows back where it was cleaned. What actually builds it can be over-spraying, a die that is too cold, hard dilution water, a mix too rich in solids or too little blow-off air, and sometimes two or more at once.

Background

Each time the die opens, a white or yellowish film in the cavity corners and along the parting line has grown a little thicker. At first it shows as a dull stain on the casting surface, but soon the dimension at that spot drifts to the edge of its tolerance and flash at the parting line increases. In the end the line has to stop for die cleaning, and production stops with it. Build-up has been reported to upset the dimensional accuracy of castings and the sealing of the die, lowering casting quality (Laudenklos & Reihmann, 2015).

A water-based release agent is almost all water, with only a small amount of active ingredients that form the film. When sprayed droplets reach the die, the water boils off and cools the die, and the remaining ingredients stick to the die face as a film (Togawa et al., 2011). The film separates casting from die, and evaporation of the water cools the die between shots (Sabau et al., 2007). Of the conditions studied, die temperature had the greatest effect on how much release agent stayed on the die face (Aoyama et al., 1991).

So build-up forms when more solids stay on the die each shot than casting and heat take away. Where heat is short, the release agent is not broken down by heat but dries with the heat that is left, and once dried it no longer fully re-emulsifies in water, so it becomes a layer as spraying is repeated (Laudenklos & Reihmann, 2015). The hypotheses below are different ways of widening this gap between what stays and what is taken away.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: mark where the layer forms on a drawing of the die, log the spray program, die temperature, dilution ratio, dilution water and blow-off settings at the time, and compare them with the release agent's technical data sheet, the TDS.

Hypothesis 1: over-spraying

Spray time and volume are usually set for the hottest spot. The die temperature range in which a water-based release agent forms a good film is narrow, so a die hotter than that range tends to be sprayed far more than needed just to cool it (Togawa et al., 2011). This happens right after spraying was increased to stop soldering, after a change of cycle time, or on lines where an operator adds spray by hand. A hot die needs a long spray phase to cool before a film can form, and the result is overspray and build-up on cooler surfaces, with lost production time and extra die maintenance (White, 2026).

Picture the week a new die is hung and its cycle is being set. Aluminium soldered at a hot spot near the gate, so spray time was raised by a few seconds and the soldering stopped. But the shallow ribs and parting line edges sprayed by the same nozzles stay wet after each shot, and within days a film has settled there in layers, with the same pattern printed on the castings.

Not everything sprayed becomes film. By one account, about a third of the sprayed droplets never reach the die, and of those that do, only part forms film while the rest goes into cooling (Togawa et al., 2011). On a cooler die, the same volume sprayed in a shorter time actually removed less heat, because the excess release agent ran off (Graff & Kallien, n.d.). The run-off gathers on lower faces and in corners, dries slowly and leaves a little solid there every shot. Raising spray pressure and duration also widens the area the release agent reaches, so spray aimed at a hot spot ends up wetting the cooler faces around it (Blowers, n.d.).

Checking starts by comparing the records with what actually happens. Match the nozzle positions, times and volumes in the spray program with the real motion, and catch each nozzle's output for a set time in a container to see whether it matches the setting. Watch whether liquid runs down the die face just after spraying ends, and whether the layer sits where the spray pattern lands. One study estimated the amount of water-based release agent film by measuring the gloss of the die surface, so gloss at fixed spots can serve for comparison (Aoyama et al., 1991).

If over-spraying is confirmed, treat cooling and release as separate jobs. Hand as much die cooling as possible to the internal cooling circuits and temperature control, and keep only as much spray as the film needs. Give hot spots their own nozzles, and cut or switch off the nozzles that reach cooler faces. Spraying in short pulses has been proposed as a way to reduce the steam barrier in front of the die so the release agent reaches it better (Sabau et al., 2007).

Hypothesis 2: die too cold

When the layer gathers in thin sections far from the gate, right beside cooling channels, early in a run or after a long stop, look at die temperature. Cutting warm-up shots short and going straight into production, winter mornings, and changes to cooling water temperature or flow all lean the same way. Say the first run on a Monday morning went into production after only a few warm-up shots. The gate side heats up quickly, but on the thin walls at the far end the spray stays white and runs every shot, and those streaks are still there in the afternoon.

A cold die drives the water off slowly. When the die is cool, the temperature difference between die and liquid is small and little evaporation takes place, so heat leaves poorly (Graff & Kallien, n.d.). One technical paper explains that below about 150°C the water cannot evaporate quickly and the active ingredients run off still as emulsion, while above about 250°C droplets boil and bounce away in the Leidenfrost effect (Togawa et al., 2011). The Leidenfrost point is the temperature that divides liquid boiling in contact with a surface from liquid floating on a vapour film, and it shifts with the liquid and the surface (Bernardin & Mudawar, 1999).

What stays behind at cold spots becomes the layer. Where the temperature is not high enough to break the release agent down by heat, it dries with the heat that remains, and the dried film does not fully re-emulsify in water (Laudenklos & Reihmann, 2015). At hot spots, on the other hand, the vapour layer makes it hard for the release agent to reach the die face (Cuadrado et al., 2025). So within one die, hot spots can solder for lack of film while cold spots build up from too much of it. The Leidenfrost point and wetting have been measured separately for each combination of lubricant and die steel between 20 and 320°C, so the temperature window for a good film has to be checked in the data for the product in use (Zabala et al., 2018).

Die temperature shows itself as soon as it is measured. Take thermal images of the die face just before and just after spraying, and see whether the build-up spots coincide with the cool ones. If the die has thermocouples, pull the temperature log against running time, and check the flow and temperature in the cooling circuits that serve the cold spots and the settings of the die temperature control unit. Compare the measured temperatures with the die temperature range the TDS recommends.

If the die is confirmed to be too cold, warm the die first. Bring it into range before production with the temperature control unit or warm-up shots, and reduce or delay cooling to the cold spots. Cut the spray that reaches them, and if the die's temperature spread is wide, choose with the supplier a release agent that forms a good film across that spread.

Hypothesis 3: hard dilution water

Suspect water hardness where dilution water comes from a well, softener regeneration gets skipped, the source water changes with the season, or the mixing tank is filled straight from plant mains. Because the same water feeds every nozzle, this kind of layer tends to appear across the whole die rather than at one spot, and it can leave traces in nozzles and pipework too. Think of the week after softener regeneration was skipped. White crust settles on the mixing tank walls and nozzle tips, the spray pattern splits to one side, and the die is covered with a rough white film instead of the usual smooth one.

Water hardness is the amount of calcium and magnesium dissolved in water. When hard water is heated, calcium carbonate settles out as a solid, and calcium in hard water reacts with soap to form scum (USGS, n.d.). On the die, the water evaporates every shot, so the minerals it carried stay behind with the release agent solids. Hard water also unsettles the emulsion itself. In a study of metalworking fluid emulsions, adding hard water salts made the emulsion particles grow, and EDTA, a chelating agent that binds calcium, was ineffective or inefficient because it interacted directly with the emulsifier (Zimmerman et al., 2004). One die-casting release agent supplier advises that high-hardness water can lead to spray nozzle plugging and in-cavity build-up (Chem-Trend, n.d.).

The first check is the total hardness of the dilution water at the mixer inlet. Measure it with test strips or a titration kit, record whether it changes with the season and the softener regeneration cycle, and look at the regeneration records and salt top-ups too. Watch for white crust on nozzle tips and tank walls, and for signs of a breaking emulsion such as cream on the surface or separating layers in the tank. Setting a sample diluted with soft water beside it makes the difference easier to see.

If hardness is high, change the dilution water first. The same supplier recommends soft water, adding that water up to about 100 ppm total hardness has been used with no adverse effects, while very pure water below 10 ppm can cause die corrosion (Chem-Trend, n.d.). So use treated water within the supplier's range rather than the purest water available. Set and record a regeneration cycle for the softener, and clean crusted nozzles, pipework and tanks before refilling.

Hypothesis 4: over-rich mix

The dilution ratio easily drifts richer without anyone noticing: when a dosing pump goes off, when mixing is done by eye, when water alone evaporates from an open tank, and when the ratio was raised to tackle soldering or sticking and never put back. After a few soldering incidents, someone turned the mixer one step richer. Soldering eased, but a few weeks later the film on the cavity floor has turned into a yellow, sticky layer, and nobody remembers touching that dial.

What hides this hypothesis is that concentration does not change cooling. In one experiment, varying the dilution between 1/20 and 1/60 left the heat removed from the die unchanged, because only a very small amount of solids is needed to lower the surface tension of water. The same experiment explains that dilution does change on-die performance, which depends on the quantity and chemistry of the solids film left once the water evaporates (Graff & Kallien, n.d.). A rich mix, then, cools just the same while leaving more solids on the die every shot. Gloss measurements on dies also confirmed that film amount varies with spray conditions, concentration among them (Aoyama et al., 1991). Wax and silicone ingredients no longer fully re-emulsify in water once dried, so the surplus carries on into a layer (Laudenklos & Reihmann, 2015).

Look at the concentration actually coming out of the spray nozzles rather than the mixer setting. Measure a sample caught at a nozzle by the method the supplier specifies, and log it beside the mixer setting and the TDS dilution ratio. Check the dosing pump's real output by catching a set volume, and look for records of topping the tank with water alone or concentrate alone. As one industry article notes, poor control of dilution makes the process inconsistent, so measuring every shift beats measuring once (Cross, 2023).

If the mix is confirmed rich, bring it back to the TDS ratio, set by a metering mixer and logged. Solve the problem that prompted the increase, such as soldering, through die temperature and nozzle layout before reaching for concentration. If the ratio must change, change it one step at a time and settle on it only after a trial that watches build-up and soldering together. Keep tanks covered so water does not evaporate.

Hypothesis 5: weak blow-off

Build-up concentrated in recesses that air reaches poorly, such as deep boss bottoms, core pin roots and the gaps between ribs, can point to the blow-off. It happens when blow time was cut to shorten the cycle, when other equipment shares the compressed air and pressure drops, when blow nozzles are blocked or bent, and when water and oil collect in the air line. Open the die the day after the blow was trimmed by about a second to meet a cycle target, and the bottoms of deep bosses and pin roots glisten with moisture, with the next spray landing on top of it.

Blow-off is the step that clears and dries the liquid left behind. Even when a water-based release agent forms its film well, some liquid remains in the cavity, and since it causes porosity, water stains on the casting surface and the risk of explosion when water meets molten metal, it is dried with blown air (Togawa et al., 2011). Film thickness has been summarised as set by spray pressure and droplet impact velocity, by adhesion and wash-off, and by the flow of cooling water and air (Sabau et al., 2007). With too little air, liquid in recesses cannot fully dry before the next shot, and as it dries it gathers its solids on that spot. A film once dried by heat does not fully re-emulsify, so the next film settles on top (Laudenklos & Reihmann, 2015).

Measure pressure right at the blow nozzle. Read it with a gauge at the moment the blow runs in production, and check how far it falls when other equipment runs at the same time. Look at blow time and sequence in the program, at nozzle blockage and aim, and at the air line drains and filters for collected water and oil. Run only the spray and blow in manual mode, stop and lock out the machine, and look for moisture still glistening in the recesses; that shows whether the wet spots match the build-up spots.

If the blow is the cause, restore the trimmed time and pressure first. Give deep recesses their own blow nozzles aimed at them, and pass the compressed air through a dryer and filters that remove water and oil. If shared equipment makes the pressure swing, a receiver tank on the blow side is one option. If cycle time has to come down, look first at cutting spray volume, so there is less liquid to dry, rather than cutting the blow.

Finding the cause

There is no need to search all five hypotheses at once. Rule them out starting with what can be measured without stopping the line. Dilution water hardness and the concentration coming out of the nozzles take a cupful of sample, blow pressure takes one gauge, and die temperature takes one pass with a thermal camera. Checking the spray program against actual output comes next.

The shape of the build-up is the next clue. Build-up on thin walls far from the gate and beside cooling channels points to a cold die; on the parting line and ribs along the spray pattern, to over-spraying; and in recesses such as boss bottoms and pin roots, to the blow-off. A thin, even coat over the whole die with white crust in nozzles and tanks as well suggests hard dilution water, and a film grown yellow, sticky and thick all over suggests a rich mix.

If that still does not settle it, run control trials that change one thing at a time. Clean the die thoroughly, then change a single condition: a fresh mix made with soft water, concentration back at the TDS ratio, a longer blow, proper warm-up, or less spray. Count how many shots it takes for the layer to become visible again at the same spots as before the change. The condition that clearly raises that count is the cause.

The final check is quality. As well as whether the layer now grows back more slowly, check against the same criteria per set output whether the problem dimensions, surface marks and parting line flash have recovered. Confirm too that cutting build-up has not left hot spots short of film so that soldering returns.

The hypotheses often overlap. More spray to cool the die chills the less hot spots further, bringing a cold die and over-spraying together, and run-off gathering in recesses loads the blow-off as well. Trying to make up for an emulsion broken by hard water with a richer ratio leaves minerals and surplus solids on the die together. In such cases, put die temperature and spray volume right first, then look at water, concentration and blow-off in turn, because while temperature and spray are unsettled, the effect of changing anything else cannot be compared fairly.

Limits and cautions

Suitable die temperature, dilution ratio, water hardness and spray and blow settings differ by release agent, alloy, die and machine, so numeric decisions follow the product's TDS and the equipment supplier's guidance. Analysing what the layer is made of or judging damage to die surface treatments is work for a laboratory and die specialists, and for dies with surface treatments, agree on cleaning methods with the die supplier first.

Safety matters too. For release agents and die cleaners, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and avoid breathing in spray mist. Water left in the cavity can explode on contact with molten metal, so never inject into a wet die (Togawa et al., 2011). Inspect or clean the die only after the machine is stopped and locked out, and wear heat-resistant gloves and eye protection against the hot die.

Sources

  1. Aoyama, S., Akase, M., & Sakamoto, K. (1991). Evaluation of lubricant film deposit on die casting die surface by measuring glossiness. Journal of Japan Institute of Light Metals, 41(1), 49–54. https://doi.org/10.2464/jilm.41.49
  2. Bernardin, J. D., & Mudawar, I. (1999). The Leidenfrost point: Experimental study and assessment of existing models. Journal of Heat Transfer, 121(4), 894–903. https://doi.org/10.1115/1.2826080
  3. Blowers, K. M. (n.d.). Optimization of die lubricant application [Master's thesis, Purdue University]. https://docs.lib.purdue.edu/dissertations/AAI10268956
  4. Chem-Trend. (n.d.). What is the recommended quality of dilution water to be used with die lubricants? Manufacturer document. Retrieved November 2026. https://chemtrend.com/faq/what-is-the-recommended-quality-of-dilution-water-to-be-used-with-die-lubricants
  5. Cross, M. (2023, October 23). Optimizing fluids and equipment for consistent die casting performance. EUROGUSS 365. https://www.euroguss.de/en/euroguss-365/2023/expert-knowledge/optimizing-fluids-and-equipment-for-consistent-die-casting-performance
  6. Cuadrado, N., Vidales, E., da Silva, M., Wajana, W., Muntada, L., Navarro, A., Beltran, L., & Vilaseca, M. (2025). Ester-based lubricant and anti-Leidenfrost additive solutions on aluminum high-pressure die-casting applications. Lubricants, 13(1), 32. https://doi.org/10.3390/lubricants13010032
  7. Graff, J. L., & Kallien, L. H. (n.d.). The effect of die lubricant spray on the thermal balance of dies. Chem-Trend, manufacturer technical paper. https://chemtrend.com/wp-content/uploads/2019/01/the_effect_of_die_lubricant_spray_on_the_thermal_balance_of_dies_en_v1.pdf
  8. Laudenklos, M., & Reihmann, M. (2015). Concentrate for producing a cooling and release agent or a cooling and lubricating agent and such cooling and release agents and cooling and lubricating agents (U.S. Patent No. 9,175,244). U.S. Patent and Trademark Office. https://patents.google.com/patent/US9175244B2/en
  9. Sabau, A. S., Hatfield, E. C., Dinwiddie, R. B., Kuwana, K., Viti, V., Hassan, M. I., & Saito, K. (2007). Assessment of computer simulation software and process data for high pressure die casting of magnesium (ORNL/TM-2007/41). Oak Ridge National Laboratory. https://doi.org/10.2172/932142
  10. Togawa, K., Ohira, H., Komatsubara, H., Kobayashi, M., Aoki, R., Hattori, T., & Butler, T. (2011). Water-free electrostatic spray for high pressure die casting [GIFA 2011 technical paper]. Manufacturer document. https://www.ultraseal-impregnation.com/us/wp-content/uploads/sites/6/2017/08/GIFA-2011-Final-Lubrolene-Technical-Paper.pdf
  11. U.S. Geological Survey [USGS]. (n.d.). Hardness of water. Water Science School. Retrieved November 2026. https://www.usgs.gov/water-science-school/science/hardness-water
  12. White, Z. (2026, March 17). Advancing the future of high-pressure diecasting. Foundry Management & Technology. https://www.foundrymag.com/molds-cores/article/55364398/advancing-the-future-of-high-pressure-diecasting-quaker-houghton
  13. Zabala, B., Igartua, A., Scarpis, V., Timelli, G., Girot, F., & Nevshupa, R. (2018). Multiparametric study of Leidenfrost point and wettability of lubricants on high-pressure die-casting dies. International Journal of Thermal Sciences, 125, 66–73. https://doi.org/10.1016/j.ijthermalsci.2017.11.014
  14. Zimmerman, J. B., Hayes, K. F., & Skerlos, S. J. (2004). Influence of ion accumulation on the emulsion stability and performance of semi-synthetic metalworking fluids. Environmental Science & Technology, 38(8), 2482–2490. https://doi.org/10.1021/es0340477

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.