KALTECKOREA

BlogApplication notes

Why do die castings show gas porosity?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Release & Process Aids

Adjusting the shot, its speed or the intensification pressure, is the usual response to rising gas porosity, but unless the source of the gas in the pores is found, the pores tend to come back. What actually lies behind them can be water left by excess spray, too little drying time after spraying, gas from release agent breakdown, a cold die, or blocked vents and weak vacuum, and sometimes two or more act at once.

Background

A machined housing shows a cluster of round holes on its cut face or in its X-ray image, and leak test rejects start to rise. Pores usually stay hidden until machining cuts the skin away or the part goes through a leak test, so the cost of casting, trimming and machining is thrown away with it. Porosity lowers pressure tightness and surface quality and can reduce strength and ductility, which makes it the main obstacle to using die castings for critical automotive parts (Piwowońska et al., 2026). Pores that hold gas swell during high-temperature solution treatment and raise blisters on the surface, so ordinary die castings are hard to heat treat at high temperature (Lumley et al., 2007).

High pressure die casting forces molten metal into a die very fast and freezes it in a short time. Gas is trapped in the metal while the melt fills the shot sleeve and the die cavity; ordinary die castings hold 10 to 50 cm³ of gas per 100 g at standard temperature and pressure, and vacuum can bring this below 10 cm³ (Piwowońska et al., 2026). Gas extracted from aluminium alloy die castings was mainly hydrogen, carbon dioxide and nitrogen, with carbon monoxide below 1%, and the amount of gas varied with the type of release agent (Tomita et al., 1981).

The gas in die casting pores is made up of air trapped during filling, hydrogen, and vapour formed as the organic release agent sprayed on the die wall breaks down (Lumley et al., 2006). The hydrogen comes mainly from water. When water meets hot aluminium it forms oxide and hydrogen, and hydrogen dissolved in the melt comes out as bubbles because the amount the metal can hold drops sharply as it freezes (Campbell, 2015). With a water-based release agent diluted for use, most of the liquid reaching the die is water, so how much water is left when the die closes can change the amount of porosity a great deal.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: log the die number, production time and location in the part for each porous casting, and compare the dilution ratio, spray volume and spray time, blow time, die temperature and vacuum level at that time with the release agent's technical data sheet, the TDS, and the process sheet.

Hypothesis 1: too much spray

Look at this hypothesis after spray time has been raised to cure soldering or poor release, when worn or clogged nozzles throw the spray to one side, and on dies with many deep ribs and bosses. The more places there are where run-off can gather, such as hollows low on the die, the closer the look. Picture the week after aluminium stuck to the die a few times and the operator raised the spray time by a step. Just before the die closes, the bottoms of the deep ribs still glisten with water, and from then on small holes start to show on the machined faces near those ribs.

More spray does not make a proportionally thicker film. In front of a hot die a vapour layer forms from evaporating water or breaking-down release agent, and it keeps the following droplets from reaching the die face, which is why spraying in short pulses, so the vapour layer can clear between them, has been proposed (Sabau et al., 2007). Liquid that fails to stick runs down and gathers in grooves and hollows, and water that has not dried by the time the die closes meets the melt and turns into hydrogen and steam. Release agent suppliers also explain that water on the die can aggravate gas porosity (Chem-Trend, n.d.). In plant trials where a coated die allowed 83 to 92% less spray, later T6 heat treatment trials indicated far less entrapped gas, although the reduction was not quantified (Midson et al., 2017).

The place to check is the cavity just before the die closes. Stop the cycle once after spraying and blowing are complete, and look for water or pooled liquid in deep ribs, at the bottom of bosses and on the lower faces of the die; film the spray to see whether liquid runs down. Measure spray volume per shot by catching each nozzle's output in a container or by comparing flow meter records, and X-ray the porous areas to see whether they line up with the spots that stayed wet. For X-ray grading of die castings, a standard with reference radiographs for each type and severity of discontinuity can be used (ASTM International, 2022).

If water is shown to remain, turn the spray volume back down. Check the volume and direction of each nozzle and replace worn or clogged ones, and on deep grooves change the spray angle or spray in short bursts so liquid does not pool. If spraying was raised because of soldering, look at the local die temperature and the type of release agent rather than adding more spray. Keep the dilution ratio within the TDS range and record every change on the process sheet.

Hypothesis 2: no time to dry

Pressure to shorten cycle time, an air blow cut short after spraying, low blow air pressure or compressed air carrying water and oil are all reasons to suspect that the water has too little time to dry. Suspicion grows if porosity rose after the production rate went up while spray volume stayed the same. Say a line took a few seconds off the cycle by shortening the blow to meet a delivery. The spray pattern and release agent are unchanged, but white steam rises near the parting line the moment the die closes.

The way a water-based release agent forms its film is also the way its water leaves. The agent builds a parting film between die and casting, and between shots its water evaporates and cools the wetted areas; even after spraying stops, the vapour layer in front of the die takes time to clear (Sabau et al., 2007). Only once the water is gone does the remaining material settle into a film, so if there is not enough time to evaporate and blow off, the die closes with water and steam still in the cavity. Gas is trapped in the metal while the melt fills the sleeve and cavity (Piwowońska et al., 2026), so steam and hydrogen from leftover water can enter the casting by the same route.

Set blow time, blow air pressure and cycle time from before and after the porosity rise side by side. Check whether steam or water shows at the parting line and in the cavity just before the die closes, and hold a dry cloth or a mirror in front of the blow nozzles to see whether the compressed air carries water or oil. Measuring the die surface temperature right after spraying and just before closing shows whether there was enough time and heat in between for the water to dry.

If the shorter blow is to blame, find the cycle time saving somewhere other than the blow. Return the blow time to what it was when there was no porosity, then shorten it step by step to find where pores come back, and service the air line drains and filters so the air comes out dry. Pulse spraying, which delivers the same amount in several short bursts, has been proposed as a way to let the vapour layer clear and get more agent onto the die (Sabau et al., 2007), so a trial of the spray method with the release agent supplier is worth running.

Hypothesis 3: breakdown gases

If porosity rose after a change of release agent type or supplier, or after the agent began to be run at a higher concentration, it is time to suspect the agent itself. The same goes for parts cast with a hot melt or a hot die. On a cold chamber machine, put the plunger lubricant applied to the plunger tip in the same group. Imagine the first week after switching to a new release agent for better release. The smoke that rises each time the die opens is thicker than before and smells different, and pores turn up all over the casting, with no link to the spots that used to stay wet.

The active ingredients of a release agent are mostly organic. In thermogravimetric analysis in air of a die casting agent made from refined oils, natural and synthetic polymers, waxes, wetting agents and emulsifiers, the agent began to volatilise at about 250 °C and broke down in five stages up to about 485 °C. The same report explains that if the agent decomposes too quickly during filling, its breakdown products can be carried into the cavity and make defects more likely (Sabau et al., 2007). In a cold chamber machine, melt poured into the sleeve evaporates and burns the lubricant on the plunger tip, and the combustion products become gas and non-metallic inclusions that can be carried into the die and trapped in the casting (Lu et al., 2025). Analyses that found the amount of gas varied with the type of release agent support this route as well (Tomita et al., 1981).

Clues to gas from the release agent lie in the change records. Match the day porosity began to rise against changes in release agent lot, type and dilution ratio, and ask the operators whether the smoke and smell at die opening changed. Pores holding gas swell into blisters at high temperature, so heating a few castings made under different conditions to the same temperature and comparing how much their surfaces blister shows which carries more gas (Lumley et al., 2007). On a cold chamber machine, also check the plunger lubricant feed rate and whether burnt residue has built up in the sleeve.

Once the cause narrows to breakdown gas, cut the amount used first. Move the dilution ratio to the lean side of the TDS range, and trim the spray so it reaches only where release is needed. If pores remain, pick a grade with less gas and smoke on thermal breakdown with the supplier and test it against the current one on the same die. Reset the plunger lubricant feed to what the sleeve actually needs, and review the shot profile too, since in the same study adjusting the slow-shot speed and acceleration to reduce air entrainment and oxide inclusions lessened the effect of the combustion products (Lu et al., 2025).

Hypothesis 4: cold die

If pores cluster in the first shots of a shift or on restart after a die change or a long stop, look at die temperature first. Winter, hard-running die cooling water and spraying that does much of the die cooling also make a cold die likely. Think of a day when only the first shots after the lunch stop are caught at X-ray inspection. Once the die has warmed up in the afternoon, pores at the same spot fall away, and the face of the die that shows up cold on a thermal image stays wet for a while after spraying.

On a cold die, sprayed water cannot boil off. A test report that measured heat flow during release agent spraying cites earlier work showing that below a surface temperature of 165 °C only a little of the liquid boils and heat leaves mainly by convection, and in its water spray tests it divided boiling into nucleate boiling from 150 to 250 °C, transition boiling from 250 to 350 °C and film boiling above 350 °C (Sabau et al., 2007). Water that does not boil stays on the die face as a thin film or droplets, and water still there when the die closes meets the melt and forms oxide and hydrogen (Campbell, 2015). So a cold die can produce the same symptom as excess spray without any change in spray volume.

Die temperature is easier to judge once it is written down as numbers. Record die surface temperature just before spraying, right after spraying and just before closing, and with a thermal camera see the cold and hot areas of the whole die in one image. Without one, measure a few fixed points with a contact thermometer in the same order every time. Sort porosity rejects by shot number and time to see whether they cluster after start-up or stops, and check the die temperature controller's set points and actual flow.

The basic remedy is to warm the die before the first shot. Preheat with the die temperature controller, and set aside a fixed number of warm-up shots after start-up and after stops. If spraying does much of the die cooling, rebalance spray volume and cooling water flow together so the die stays hot enough after spraying for the water to dry. The right die temperature range differs by alloy, part and release agent, so follow the TDS and the die design conditions.

Hypothesis 5: trapped air

The last areas to fill, the spots near overflows and vents and the ends of thick bosses are where air is most likely to be left behind. Suspect venting when pores cluster there and the vents have gone uncleaned for a long time, vacuum valves and filters are past their service date, or the vacuum line leaks somewhere. On a vacuum die casting line, the vacuum reading sometimes falls more slowly than usual for several days running. Open the vent block, and the inside of its narrow channels is coated with release agent residue and thin flakes of aluminium.

While the melt rushes in, the air in the sleeve and cavity has to escape through vents or vacuum channels, and air that cannot escape is trapped in the metal as pores. In a study of two-stage vacuum die casting that evacuated the cavity and sleeve together to 19 mbar, both the volume fraction and the size of pores fell compared with conventional die casting (Dong et al., 2019), and a study comparing 3D vents with a mechanical valve also found that gas porosity and machine downtime dropped markedly (Altuncu et al., 2019). Release agent can narrow the vent path too. Some of the agent that misses the die lands in the vents and leaves a film as the water dries, and because this film is not fully cleared with each shot, it can restrict the path for escaping gas (Chem-Trend, n.d.).

Start by locating the pores. Mark their positions from X-ray images or sections and see whether they coincide with the last-to-fill areas of the die or with areas far from the vents, then open the vent blocks and overflow channels to check for release agent residue, aluminium flakes and blockages. On a vacuum line, compare the vacuum curve logged for each shot with the curves from when there was no porosity. If the vacuum reaches its target late or never gets all the way down, look for leaks at valves, filters, hoses and the sealing faces of sleeve and die.

Clean vents and vacuum channels every fixed number of shots, before they block rather than after. Keep service records for vacuum filters and valves. If release agent keeps building up in the vents, reduce or redirect the spray near them. Changing vent position and size is a die design matter, so review pore locations and filling simulation results with the die maker.

Finding the cause

Five hypotheses do not call for five investigations at once. Rule them out starting with what records and eyes can show straight away. Spray time, blow time, dilution ratio, die temperature and vacuum level are already in the machine and the records, and water in the cavity and the state of the vents can be seen by stopping the cycle once. Trials of a different release agent and die modifications take time, so they come after.

First make sure the holes are gas pores. In a study that classified die casting pores by 3D X-ray tomography, gas pores were near round and shrinkage pores very complex in shape, while mixed pores looked like gas pores but carried protrusions and long tails (Wan et al., 2014). Shrinkage pores call for a look at conditions that govern solidification, such as wall thickness, gating and intensification, rather than the release agent.

For round gas pores, place and timing are the next clues. Pores gathered in grooves and rib bottoms that stayed wet point to spray volume; pores that rose after the cycle was shortened or the blow cut point to drying time; and pores clustered after start-up or stops point to die temperature. Pores near the last-to-fill areas and the vents point to venting and vacuum, and pores scattered across the casting that coincide with a change of release agent point to breakdown gas.

If that still does not settle it, run control trials that change one thing at a time. On the same die, cut only the spray volume, then lengthen only the blow time, then add warm-up shots, and compare with the state just after cleaning the vents. Grade the same locations against the same reference radiographs as before the change (ASTM International, 2022). The final check uses the method the customer actually rejects parts by, such as a leak test or inspection of machined faces, and the job is done only when a set quantity made under the new condition shows the reject rate back where it was.

The hypotheses are tangled together. Raising the spray to cure soldering leaves water behind, the same spray cools the die so the water dries more slowly, and agent that runs off builds up in the vents and narrows the venting too. It is better to settle water and temperature first. While the amount of water left on the die varies from shot to shot, the effect of changing the release agent or the vents is lost in that variation.

Limits and cautions

Suitable dilution ratio, spray volume, blow time, die temperature and vacuum level differ by alloy, part shape, machine and release agent, so numeric decisions follow the release agent's TDS and the machine and die suppliers' guidance. Porosity also has causes unrelated to the release agent. Melt that carries too much dissolved hydrogen from the start is a melting and degassing matter, and shrinkage pores from thick sections contracting as they freeze are a die and gating design matter, so review them with the people responsible. Judge parts where pressure tightness or strength matters by X-ray, tomography or leak test results, and do not release them on floor judgement alone.

Safety matters too. For release agents and plunger lubricants, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and check local exhaust around machines that give off heavy breakdown smoke. Inspect or clean the cavity and vents only after the machine is stopped and locked out, and wear heat-resistant gloves and a face shield against the hot die and metal splash. Keep wet tools and damp material away from molten metal.

Sources

  1. Altuncu, E., Doğan, A., & Ekmen, N. (2019). Performance evaluation of different air venting methods on high pressure aluminum die casting process. Acta Physica Polonica A, 135(4), 664–667. https://doi.org/10.12693/APhysPolA.135.664
  2. ASTM International. (2022). ASTM E505-22, Standard reference radiographs for inspection of aluminum and magnesium die castings. https://store.astm.org/e0505-22.html
  3. Campbell, J. (2015). Complete casting handbook: Metal casting processes, metallurgy, techniques and design (2nd ed.). Butterworth-Heinemann.
  4. Chem-Trend. (n.d.). Porosity. Manufacturer technical information. Retrieved November 2026. https://de.chemtrend.com/problem/porosity/?lang=en
  5. Dong, X., Zhu, X., & Ji, S. (2019). Effect of super vacuum assisted high pressure die casting on the repeatability of mechanical properties of Al-Si-Mg-Mn die-cast alloys. Journal of Materials Processing Technology, 266, 105–113. https://doi.org/10.1016/j.jmatprotec.2018.10.030
  6. Lu, J., Lordan, E., Zhang, Y., Fan, Z., & Dou, K. (2025). Influence of piston lubricant on the distribution of defects in cold chamber high pressure die casting. Lubricants, 13(3), 99. https://doi.org/10.3390/lubricants13030099
  7. Lumley, R. N., O'Donnell, R. G., Gunasegaram, D. R., & Givord, M. (2006). New heat treatment for Al high pressure die-castings. Heat Treating Progress, September/October 2006.
  8. Lumley, R. N., O'Donnell, R. G., Gunasegaram, D. R., & Givord, M. (2007). Heat treatment of high-pressure die castings. Metallurgical and Materials Transactions A, 38(10), 2564–2574. https://doi.org/10.1007/s11661-007-9285-4
  9. Midson, S., Korenyi-Both, A., & Kaufman, M. (2017). Casting solutions for readiness: Lube-free die casting [Report]. Colorado School of Mines. https://apps.dtic.mil/sti/pdfs/AD1098829.pdf
  10. Piwowońska, J., Białoń, J., & Dudek, P. (2026). Optimization of the high pressure die-casting process to reduce porosity. Archives of Foundry Engineering, 26(2), 15–20. https://doi.org/10.24425/afe.2026.157985
  11. Sabau, A. S., Hatfield, E. C., Dinwiddie, R. B., Kuwana, K., Viti, V., Hassan, M. I., & Saito, K. (2007). Assessment of computer simulation software and process data for high pressure die casting of magnesium (ORNL/TM-2007/41). Oak Ridge National Laboratory. https://info.ornl.gov/sites/publications/files/Pub8532.pdf
  12. Tomita, K., Taniyama, H., Imabayashi, M., & Iwamura, H. (1981). Gases in aluminum alloy pressure die castings. Journal of Japan Institute of Light Metals, 31(3), 186–194. https://doi.org/10.2464/jilm.31.186
  13. Wan, Q., Zhao, H., & Zou, C. (2014). Effect of micro-porosities on fatigue behavior in aluminum die castings by 3D X-ray tomography inspection. ISIJ International, 54(3), 511–515. https://doi.org/10.2355/isijinternational.54.511

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.