Raising cleaner concentration or washing longer is the usual response when deep-drawing oil will not wash off, but during forming the oil reacts with the metal and changes with heat, and it keeps changing while it waits to be cleaned, so harder washing without knowing what is left may still leave it. What actually lies behind it can be reaction films from extreme pressure additives such as chlorinated paraffin, solid fillers such as calcium carbonate, a film oxidised by forming heat, a long wait before cleaning, or a cleaner and temperature that do not suit the oil, and sometimes two or more at once.

Background

Deep-drawn cups and housings go through the washer, and when they come out a film of oil or white stains remains at the bottom corners and on the walls. Passed on as they are, they give small crater-like marks in paint, plating that lifts, or smoke and soot at the weld. Washing two or three times turns the washer into a bottleneck, and parts that will not come clean have to be wiped by hand or scrapped.

Deep-drawing oil is made to withstand high pressure and heat. On a mineral oil base it carries extreme pressure, or EP, additives that react with the metal surface to prevent welding, emulsifiers that help residue wash off in cleaning, and corrosion inhibitors that protect parts in storage, among others (DEPA, 2005). During forming, fresh sheet surface is exposed and heated, and part of the lubricant reacts and changes on it. What enters the washer is therefore not the oil that was applied. That is why a forming lubricant has to suit the final degreasing step as well as lubricate (Aha et al., 2021).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep parts that stayed oily after cleaning together with parts straight off the press and parts before cleaning, log the lubricant and cleaner used, the time from forming to cleaning and the bath temperature and concentration, and compare them with the technical data sheets, the TDS, of both products.

Hypothesis 1: EP reaction films

Heavy drawing oils rich in EP additives are used for sheets that stick to tooling, such as stainless steel, for thick sheet and for deep draws. Chlorinated paraffin oils have often been used to form materials prone to galling, such as high-strength steel, stainless steel and titanium (Bay et al., 2010). Hold a cleaned stainless cup up to the light: the flat bottom is clean, but a thin iridescent or pale brown film remains only on the wall that passed the die radius and at the bottom corners. Rubbing with a cloth does not shift it.

A reaction film is not oil but a new compound made by metal and additive. EP additives bond chemically with the metal when the local temperature at the contact rises, forming a surface film that keeps metal from welding and scoring (DEPA, 2005). In a study of ironing stainless steel, chlorinated paraffin reacted evenly with iron, chromium and nickel, and depth profiling suggested that the chlorinated lubricant promoted a thick oxide layer (Petrushina et al., 2000). The reaction happens where pressure and heat are high, so the film tends to gather at places such as the die radius and the corners. Alkaline cleaners and surfactants are built to dissolve and lift oil, so reaction products and oxide bonded to the metal surface may not come away as easily as oil does.

Where the film sits is the clue. On a cleaned part, mark where colour remains and where the water film breaks when water is poured over it, and see whether those places match high-pressure zones such as the wall past the die radius and the corners. If flat faces are clean and only those zones keep a film, it points to reaction films. Check the type of EP additive in the drawing oil's TDS, and if needed have a laboratory run surface analysis to see whether the film contains chlorine or sulfur.

If reaction films look likely, go back to the choice of lubricant. Agree with the supplier to use only as much EP additive as the draw actually needs, and keep heavy oil for the hardest operations or areas. A Danish project searching for alternative lubricants likewise made degreasing of formed parts with alkaline cleaners one of its selection criteria (DEPA, 2005). For films already formed, work out removal conditions with the cleaner supplier by trialling cleaner types and temperatures, and make those conditions the cleaning standard.

Hypothesis 2: solid fillers remain

Drawing compounds or pastes with solid particles, and oils with calcium components, are used to protect tooling in deep, severe draws, and calcium carbonate is also being examined as a lubricant additive to replace hazardous chemicals such as chlorinated paraffins (Arinbjarnar et al., 2024). Run a fingertip along the recessed bottom corner of a cleaned part and white powder comes off, and white residue has collected round holes and in folds of the flange. Once dry, the whole surface looks hazy.

Particles such as calcium carbonate dissolve in neither water nor oil. So even after the cleaner dissolves the oil, the particles stay in the valleys of surface roughness and in recesses, and only force such as a jet of water or a brush moves them. In sheet forming tests, lubricant mixed with calcium carbonate did better than commercial forming oils in wear testing but worse in weld load testing, cleaned off less easily, and left scratches on the formed parts (Arinbjarnar et al., 2024). Calcium can stay on the surface even when not added as particles: an oil combining a sulfur EP additive with calcium and zinc components formed sulfide and calcium carbonate on the surface of stainless steel products, where they acted as the lubricating film (Takaki et al., 2018). The film that helped forming becomes residue to be removed in cleaning.

The identity of the powder is easy to check. Scrape together white powder left after cleaning and add a drop of dilute acid; if it fizzes, it is a carbonate. Check the lubricant's TDS for solid and calcium components, and see whether the powder gathers where the wash flow is weak, such as recesses and round holes. Look at the surface under a magnifier for particles lodged in the roughness valleys.

If solid particles are the culprit, add physical force to the cleaning. Aim spray pressure and nozzles at the recesses, and for immersion cleaning consider agitation or ultrasonics. An acid rinse dissolves carbonates but can attack the metal surface or invite rust, so use one only after setting conditions with the cleaner supplier. The sheet forming study concluded that solid particles as lubricant additives should be confined to operations where abrasive wear is the main problem, so for parts that are hard to clean, review with the supplier a switch to a lubricant without solids (Arinbjarnar et al., 2024).

Hypothesis 3: film oxidised by heat

This hypothesis gains weight for parts drawn deep and fast, tools running without a break, summer afternoons, and drawing oils that contain vegetable oils or their esters. Late in the afternoon a cup fresh from the press feels warm even through a glove, and the oil left at the bottom corners and on the walls looks darker than on morning parts and comes off sticky on the hand. After cleaning, yellowish stains remain only in those places.

Despite the name, room-temperature forming is hot at the contact. A study modelling the room-temperature forming of high-strength sheet predicted temperatures of up to 108 °C in the sheet and 181 °C in the tool, and validated this experimentally (Pereira & Rolfe, 2014). The heat comes from plastic and frictional work and drives tool temperature up from the start of a run (Aha et al., 2021). Vegetable oils lubricate well and are biodegradable, but their main weakness is poor oxidative and thermal stability; they undergo autoxidation, a self-sustaining reaction with oxygen in the air, and as oxidation proceeds, molecules can link up, raising viscosity and leaving sticky products (Fox & Stachowiak, 2007). Oil oxidised this way may not come off under cleaning set up for fresh oil.

Separate the hot places from the cool ones. Measure the temperature of corners and flat faces on freshly formed parts with an infrared thermometer, and mark whether stains after cleaning coincide with the hot spots. Pull and clean parts from different times of the run, and it shows whether stains concentrate on afternoon parts from a heated tool. Send residue from the stained areas to a laboratory with fresh drawing oil to compare how far oxidation has gone.

There are two directions. One is to reduce heat: improve tool cooling and adjust an excessive press speed. The other is to choose oil that stands up to heat. Ways to assess and improve the oxidation stability of vegetable oils have been studied (Fox & Stachowiak, 2007). Choose with the supplier a product backed by oxidation stability data, and test its cleanability on real parts before switching. Not leaving formed parts stacked hot for long also helps.

Hypothesis 4: long wait to clean

The gap between forming and cleaning opens for several reasons: cleaning is sent out to a subcontractor, stock is built up to suit the schedule of the next process, a holiday or weekend intervenes, or parts are kept in a hot or sunlit store. Parts drawn on a Friday afternoon and stacked in crates reach the washer only midway through the next week. Under the same cleaning conditions, they keep more stains than parts that used to be cleaned the same day.

The oil film keeps changing while it waits for the washer. Oxidation by oxygen in the air continues after forming, and oils with vegetable components, being weaker against oxidation and heat, can thicken and turn sticky over time (Fox & Stachowiak, 2007). Reaction films and oxide formed by EP additives also stay bonded to the surface all the while. The mineral oil in a drawing oil is also meant to leave a corrosion-protecting film while parts are stored (DEPA, 2005). A film made to last and protect the part can work against cleaning.

Splitting one lot in two is the cleanest test. Divide parts formed in one run, clean half straight away and the rest after the usual storage, and compare the two with the water-break test and the weight difference before and after cleaning. From routine records, match forming and cleaning dates lot by lot and see whether stains cluster in lots that waited longer. Log the storage temperature as well.

If waiting is the problem, set an upper limit on the time from forming to cleaning. Clean parts in the order they were formed, and if they must wait, keep them covered somewhere cool and out of the sun. Where the time is hard to shorten, as with subcontracted cleaning, choose with the suppliers a lubricant and cleaner pair proven to clean well after storage.

Hypothesis 5: cleaner or temperature

Look at cleaning first after a change of cleaner or a lower wash temperature, when the bath is topped up without measuring concentration, when oil floats on a bath left too long unchanged, and after a switch from chlorinated solvent cleaning to aqueous cleaning. The month the bath set point was lowered to save on electricity is one such case. Flat faces come out clean, but oily residue remains in recessed bottom corners and inside holes, and an oil film floats on the bath.

Cleaning is the cleaner, temperature, time and force working together. A study of carbon steel surface cleaning reports that cleaning efficiency varies with alkali and surfactant concentration, temperature and stirring, and that higher temperature lowers the viscosity of the soil and speeds up the reactions (Mihis et al., 2021). The more viscous the drawing oil, the less readily it flows out of recesses as the temperature drops. The type of cleaner has to fit too. In developing forming lubricants, the final degreasing step counts among the requirements a lubricant must meet (Aha et al., 2021). When lubricant and cleaner do not suit each other, some residue can remain even at higher concentration and temperature, and when oil builds up in the bath, floating oil can redeposit on parts as they are lifted out.

Cleaning results show at once in the water-break test. Pouring water over a cleaned and rinsed part to see whether an unbroken film covers it can detect even molecular layers of hydrophobic contamination, but the test loses much of its sensitivity on rough or porous surfaces and is a qualitative go or no-go check (ASTM International, 2021). Measure bath temperature and concentration every shift against the range in the cleaner's TDS, and record how much oil floats on the bath and when it was last changed. On a spray washer, check nozzles for clogging and pressure as well.

Choose cleaner and lubricant as a pair. When changing the lubricant, clean real parts with the current cleaner, and when changing the cleaner, with the current lubricant, and first confirm that they pass the water-break test. Set standards for bath temperature and concentration ranges, bath change intervals and how floating oil is skimmed, and put any oil skimmer on the maintenance list. The type of stirring also changes cleaning efficiency, so for parts with many recesses, adjust agitation or spray direction at the same time (Mihis et al., 2021).

Finding the cause

To separate the causes, start with the checks that take least effort. Bath temperature and concentration, the time from forming to cleaning, and the EP and solid components of the lubricant can mostly be confirmed from the records and the TDS alone. Work that needs a laboratory, such as surface analysis or oxidation comparison, comes after.

Where the residue sits is the first clue. A thin film only in high-pressure zones such as the wall past the die radius and the corners points to EP reaction films; white powder gathering in recesses and round holes to solid fillers; and yellowish, sticky stains where the part ran hot to a film oxidised by forming heat. If an oily film remains everywhere regardless of location, look first at the cleaner and temperature.

Next comes timing. Stains clustering in lots that waited long point to the wait; on afternoon parts from long runs, to forming heat; and from the time the cleaner or wash temperature changed, to cleaning. If they coincide with a lubricant change, check the new lubricant's EP and solid components.

When the clues conflict, separate them with control trials. Split parts from one lot into cleaned at once versus after storage, cleaned at the usual versus a higher temperature, and cleaned with the current versus another cleaner, keeping to one changed condition at a time. Compare results on the same basis with the water-break test and the weight difference before and after cleaning, and count the job done only when paint or plating defects in the next process have recovered.

Hypotheses can interlock. Oil rich in EP additives forms reaction films where it runs hot, the same heat speeds up oxidation of the oil, and if the parts are then stacked for a long time, the film can change further while still on them. A low wash temperature lets all of these films stay more readily. In such cases, first return cleaning conditions to standard to give a sound basis for comparison, then look in turn at waiting time, forming heat and lubricant components, because while cleaning conditions are unsettled the effect of changing anything else cannot be told apart.

Limits and cautions

Suitable EP additives and amounts, bath temperature and concentration, and how long parts may wait before cleaning differ by material, severity of draw, next process, lubricant and cleaner, so numeric decisions follow the TDS of both products and the cleanliness standard of the next process. Surface analysis and judging oxidation are laboratory work, and for products with strict residue limits, such as medical devices or food containers, do not decide on the floor water-break test alone; confirm with the cleanliness test set by the quality engineer.

Safety and regulation matter too. The U.S. Environmental Protection Agency has issued a rule under the Toxic Substances Control Act covering short-chain chlorinated paraffins, which are used as lubricants and coolants in metal cutting and forming, and continues to evaluate medium- and long-chain chlorinated paraffins as raising similar concerns, so check local regulations when using or replacing chlorinated drawing oils (EPA, n.d.). Follow the safety data sheet, the SDS, for protective equipment and ventilation with cleaners and acid rinses, and guard against burns at hot baths. Limit exposure to metalworking fluids such as drawing oils, which can harm health through skin contact and through breathing in mist (OSHA, n.d.).

Sources

  1. Aha, B., Hettich, D., Veldhuis, M., & Filzek, J. (2021). Higher productivity in forming high-alloyed steel by temperature insensitive friction behavior. ESAFORM 2021: 24th International Conference on Material Forming. https://doi.org/10.25518/esaform21.2075
  2. Arinbjarnar, Ú., Moghadam, M., & Nielsen, C. V. (2024). Performance of inert particles as lubricant additives compared to fully formulated industrial forming oils in sheet metal forming. Discover Mechanical Engineering, 3(1), 6. https://doi.org/10.1007/s44245-024-00037-8
  3. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  4. Bay, N., Azushima, A., Groche, P., Ishibashi, I., Merklein, M., Morishita, M., Nakamura, T., Schmid, S., & Yoshida, M. (2010). Environmentally benign tribo-systems for metal forming. CIRP Annals, 59(2), 760–780. https://doi.org/10.1016/j.cirp.2010.05.007
  5. Danish Environmental Protection Agency [DEPA]. (2005). Mapping and development of alternatives to chlorinated lubricants in the metal industry (KLORPARAFRI). Environmental Project No. 1039. https://www2.mst.dk/udgiv/publications/2005/87-7614-807-6/html/default_eng.htm
  6. Fox, N. J., & Stachowiak, G. W. (2007). Vegetable oil-based lubricants—A review of oxidation. Tribology International, 40(7), 1035–1046. https://doi.org/10.1016/j.triboint.2006.10.001
  7. Mihis, A., Danciu, V., Salagean, C. A., Székely, I., Racolta-Paina, M. V., Tripon, S. C., Cotet, L. C., Magyari, K., & Baia, L. (2021). The effect of alkali and surfactant concentration, temperature and stirring on the cleaning efficiency of the carbon steel surface. Studia Universitatis Babeș-Bolyai Physica, 66(1–2), 79–90. https://doi.org/10.24193/subbphys.2021.08
  8. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids
  9. Pereira, M. P., & Rolfe, B. F. (2014). Temperature conditions during 'cold' sheet metal stamping. Journal of Materials Processing Technology, 214(8), 1749–1758. https://doi.org/10.1016/j.jmatprotec.2014.03.020
  10. Petrushina, I. M., Christensen, E., Bergqvist, R. S., Møller, P. B., Bjerrum, N. J., Høj, J., Kann, G., & Chorkendorff, I. (2000). On the chemical nature of boundary lubrication of stainless steel by chlorine- and sulfur-containing EP-additives. Wear, 246(1–2), 98–105. https://doi.org/10.1016/S0043-1648(00)00503-2
  11. Takaki, T., Kitamura, K., & Shibata, J. (2018). Development of chloride-free oil with sulfur-based EP additive for cold forming of stainless steel. Mechanical Engineering Journal, 5(2), 17-00449. https://doi.org/10.1299/mej.17-00449
  12. U.S. Environmental Protection Agency [EPA]. (n.d.). Risk management for short-chain chlorinated paraffins. Retrieved November 2026. https://www.epa.gov/assessing-and-managing-chemicals-under-tsca/risk-management-short-chain-chlorinated-paraffins

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.