It is easy to assume that a dry film also keeps rust away, but the more lubricating pigment a film carries, the lower its friction and the weaker its corrosion resistance tend to be. What actually lets rust through can be a porous film, galvanic attack driven by graphite in the film, poor pretreatment, a thin film or surfaces wetted by damp and condensation, and sometimes two or more at once.

Background

You lift a box of parts out of storage onto the assembly line and find red spots rising here and there through the dark grey dry film. One box is clean, another has rust on half its parts. Rusted parts are rejected on appearance, or the film has to be stripped and pretreatment started again, so time and cost are spent twice. Parts already assembled and shipped may need taking apart and replacing, and rust on a sliding face can lift the film at that spot.

A dry film is often called slippery paint. It is a film in which lubricating pigments such as molybdenum disulfide, graphite or PTFE are held on the metal by a binder such as a resin, and over 95% of dry films in commercial use are of this resin-bonded kind. A formulation with a low pigment-to-binder ratio is glossy, hard and resists corrosion well but has higher friction, while a high ratio gives low friction with a dull, powdery look and less corrosion resistance. So choosing a film means weighing corrosion behaviour, including susceptibility to galvanic corrosion, alongside friction (Gresham, 2003).

Rust advances only when water and oxygen reach the metal surface together. Atmospheric corrosion happens while the surface is wet with a thin film of water, and the international standard estimates this time of wetness as the hours above 80% relative humidity and above 0 °C (ISO, 2012). Even a military specification for a heat-cured, corrosion-inhibiting dry film asks only that, on phosphated steel panels after 100 hours of 5% salt spray, each panel shows no more than three rust spots, none larger than 1.0 mm across (DoD, 2013). A dry film can slow rust, but it is not a film that shuts out water and oxygen entirely.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: lay rusted and clean parts side by side, note where the rust sits, the day it was first seen and where the parts were stored, then compare the pretreatment, thickness and cure that the film's technical data sheet, the TDS, calls for with the actual work records.

Hypothesis 1: porous film

Look at this hypothesis first with formulations loaded with lubricating pigment to push friction as low as possible, with films dried at room temperature without an oven, and with films sprayed thin in a single pass. The same goes when the film was chosen for sliding rather than for corrosion protection. Look at a pin coated with a dull, powdery film under a magnifier. The film seems to cover evenly, yet the rust has not gathered in one place; it has come up as pinpoint spots scattered over the whole face.

A dry film is a film in which a binder holds lubricating pigment powder. When the binder fills all the spaces between pigment particles, the film becomes a continuous polymer layer, but when there is so much pigment that binder runs short, gaps remain between the particles. In paints it was shown long ago that once pigment passes the limit the binder can fully wrap, the critical pigment volume concentration, the film's properties change abruptly (Asbeck & Van Loo, 1949). When the gaps link up, water and oxygen find a path down to the metal without passing through binder, and even without gaps a polymer film lets some water and oxygen through, to a degree set by the polymer's structure (Sangaj & Malshe, 2004). Such gaps are one way to understand the industry account that a dry film with a high pigment-to-binder ratio resists corrosion less (Gresham, 2003). If the gaps run through the whole film, rust would be expected to come up over the whole face rather than gather at edges or scratches.

Begin with how the rust is spread on parts from the same lot. If spots are scattered over flat faces regardless of edges or scratches, gaps in the film are worth suspecting. Check in the TDS whether the film is a corrosion-inhibiting grade and whether it states a pigment-to-binder ratio or salt spray results, and compare the cure temperature and time with the records. If formulations need comparing, make test panels with the same pretreatment and thickness and put them in the salt spray cabinet together. The standard itself notes that salt spray results alone seldom predict life in real environments, so use it as a comparison that ranks them (ASTM International, 2019).

If a porous film looks to be the cause, choose the formulation again. Where corrosion protection matters as much as sliding, review with the supplier a grade with corrosion-inhibiting additives or a lower pigment ratio, and check how friction shifts with it. If an air-dry grade was in use, see whether a heat-cured grade can replace it. Rather than building the film thick in one pass, spray several thin coats within the set number so the gaps do not line up, and hold the cure to the TDS temperature and time.

Hypothesis 2: graphite in film

This hypothesis comes up when a graphite-containing film is applied to aluminium or steel parts and those parts sit where chlorides reach them, such as sea air, winter de-icing salt or salty wash water. Also check it when a graphite grade was chosen for high-temperature use, or when the same film starts being used on parts of a different metal. Say boxes of aluminium brackets stood for a few weeks in the yard of a plant near the coast. White powder has swelled up along the edges of the grey film and along scratch lines, and where the powder is brushed off, small pits are left.

Graphite is a lubricating pigment and also an electrical conductor, standing on the noble side of aluminium and steel. When a film of salty water wets graphite and metal together, the two form a cell: the metal becomes the anode and dissolves, while dissolved oxygen is reduced on the graphite. In tests pairing aluminium with graphite fibre, silicon carbide or titanium diboride, galvanic corrosion was high in aerated chloride solutions, the corrosion rate of aluminium coupled to graphite came out about 30 times that of aluminium coupled to silicon carbide or titanium diboride, and in deaerated solution galvanic corrosion was negligible even with chloride present (Hihara & Latanision, 1992). A study that varied the area ratio between an aluminium alloy and graphite found that the ratio changed the very form of the attack, between localised corrosion and broader dissolution (Coelho et al., 2018). For these reasons graphite is known as a pigment that promotes galvanic corrosion, and the military specification for heat-cured corrosion-inhibiting films excludes graphite from the formulation altogether (Gresham, 2003; DoD, 2013).

Check the ingredients first. Look in the TDS and the safety data sheet, the SDS, for graphite or carbon, and compare the rust pattern with that of the same part coated with a graphite-free film. See whether rust gathers at film edges, scratches and joints with other metals, where graphite and bare metal can be linked by a film of water, and on aluminium whether there are white corrosion products and pits. Whether a film touching aluminium causes galvanic corrosion at high humidity can be checked separately with the standard test method for dry films (ASTM International, 2026).

If graphite is to blame, moving to a graphite-free formulation is the most direct route. Review with the supplier a corrosion-inhibiting grade pigmented with molybdenum disulfide or PTFE, and if graphite was chosen because the part runs hot, check the temperature limit of the replacement too. Give aluminium parts an underlayer such as anodising beneath the film, and if a graphite film must stay, change storage and packing so chlorides cannot reach it. Rework any jigs or tools that scratch the film during assembly as well.

Hypothesis 3: poor pretreatment

Suspect pretreatment when the film was sprayed straight after degreasing, when blasting was done but phosphating skipped, or when the process was cut back after a change of coating subcontractor. The same applies when parts sat for a long time after pretreatment before coating because of a rush order. Think of lots coated with the same film to the same thickness, where only those arriving after a change of subcontractor show more rust in storage. Scrape away a little film and bare metallic shine shows underneath instead of a grey crystalline layer.

Pretreatment does two jobs. One is to remove oil, rust and oxide and roughen the surface so the film has something to hold; the other is to put one more layer between metal and film that rust does not spread through easily. A phosphate coating on steel is a crystalline conversion coating formed as the metal surface reacts with a phosphate solution, used as a base that helps the coating above it adhere and slows rust (Narayanan, 2005). The military specification mentioned earlier likewise has test panels grit blasted and then phosphated at 11 to 22 g per square metre before the film goes on (DoD, 2013). Without that underlayer, water entering through the film reaches bare metal at once, and rust creeps sideways under the film and lifts it. One industry review puts 80% of dry film failures down to poor surface pretreatment or faulty application, and in a wear life test it describes, a specimen that was only degreased failed as soon as load was applied, while one degreased, blasted and phosphated lasted over 30 times longer than one only blasted (Gresham, 2003).

Look at the work records and under the film together. Check whether degreasing, blasting and phosphating were each done and how much time passed between pretreatment and coating, then scrape a little film off one or two rusted parts with a knife to see whether a grey or black crystalline layer or bare metal lies beneath. If rust has crept under the film and lifted it like a blister, or the film comes away easily on tape, suspect the underlayer and adhesion. If the subcontractor changed, lay the process sheets from before and after side by side and find the missing step.

For steel parts, fix the sequence of degreasing, blasting and phosphating before coating in the process sheet, and measure phosphate coating weight by stripping a set area and weighing the difference, keeping it within the TDS or specification range. For aluminium, use anodising or a conversion coating as the underlayer. Do not handle pretreated parts with bare hands, and coat them before the surface picks up dirt or moisture again. Where coating is subcontracted, write these steps and the records into the purchase specification.

Hypothesis 4: thin film

Check film thickness on threads, edges, bore interiors and deep grooves where spray reaches poorly, and on parts given a single pass. The same goes when the film was kept thin on purpose for a fit, or straight after a change of operator or work on the spray equipment. Take bolts with dry film on the threads, brought out of a damp store: the rust runs as a fine line along the thread crests rather than over the shank, and the flat top of the head on the same bolt is clean.

Film thickness is a value held in a narrow band between sliding and rust. Dry films are kept far thinner than ordinary paint, usually in a range of 0.0002 to 0.0005 inch for the best lubrication and wear, but the best corrosion resistance may need a thicker film, so the two have to be traded off (Gresham, 2003). The military specification sets thickness after cure at 0.008 to 0.013 mm, with no reading under 0.005 mm or over 0.018 mm, measured with the gauge zeroed on the blasted profile, and allows no more than three coats (DoD, 2013). The water and oxygen passing through a polymer film increase as the film gets thinner (Sangaj & Malshe, 2004), so the thinnest spots rust first. Where film drains away easily, such as peaks of the blast profile or thread crests, those spots alone can be thin even when the average thickness is right.

Thickness is known only by measuring it. Measure film on steel with a magnetic gauge and film on aluminium with an eddy current gauge, following the standard practice for method and gauge checks (ASTM International, 2022). Take readings at many points on a part, not only on flat faces but at edges, near threads and at bore entries, and compare thickness where rust appeared with where it did not. For threads and bores the probe cannot reach, cut and section a test panel or part sprayed under the same conditions. If rust follows only the thin spots, this hypothesis gains weight.

Once thin spots are confirmed, change how the film is applied. Alter spray angle, distance and how parts are hung so the film reaches threads and edges evenly, and build it up in several thin coats within the number the TDS allows. Where a fit rules out a thicker film, take load off the thin film by making sure of pretreatment or by using a corrosion-inhibiting grade. Record thickness at set points for every lot.

Hypothesis 5: damp surfaces

Look at damp when rust increases in the rainy season, in unheated stores, in seasons with large swings between day and night temperatures, on parts packed before they dried after washing, or inside boxes tightly wrapped in plastic. Parts moved from a cold place to a warm, humid one are no different. On a winter morning, a box that spent the night on a truck outside is brought into the warm assembly hall and opened at once. The part surfaces quickly mist over, and a few days later rust spots show first on the top layer of parts.

Iron rusts suddenly faster once the air reaches a certain humidity. A classic study of the atmospheric corrosion of iron found that rusting rose sharply above a critical relative humidity, and that pollutants such as sulphur dioxide and airborne particles made it worse (Vernon, 1935). This is also why the time of wetness mentioned earlier is estimated from relative humidity. Condensation acts more directly. When the metal surface is colder than the dew point of the surrounding air, water vapour condenses on it, and that water passes through gaps and thin spots in the film to the metal. The standard for judging the risk of condensation before painting likewise works out the dew point from air temperature and relative humidity and compares it with the steel surface temperature (ISO, 2017). With molybdenum disulfide films there is one more factor. In tests under humid conditions, moisture in contact with molybdenum disulfide formed acids that corroded the steel specimens, though that result came from powder used without a binder (Peterson & Johnson, 1953).

Start by gathering temperature and humidity records. Place data loggers in storage areas and along the transport route, and look at relative humidity and temperature swings around the day the rust was first seen. When moving parts or opening packs, measure surface temperature and compare it with the dew point of the air there. If rust gathers on the top layer of a box, in boxes near walls or floors, or where water drop marks sit inside the packing, suspect condensation; if it is spread evenly across many lots and parts, suspect long spells of high humidity. Check drying conditions after washing and when parts were packed as well.

If condensation is the cause, the key is to remove the moments when parts are colder than the surrounding air. Do not leave boxes brought in from the cold open; let them reach room temperature closed, then open them. Lower relative humidity in the store with dehumidifying or ventilation, and keep boxes off floors and away from outside walls. Pack washed parts only once fully dry, and consider desiccant or vapour corrosion inhibitor packing inside the pack. For parts going into long storage, weigh whether to add a separate rust preventive over the film against the part's sliding duty.

Finding the cause

Five hypotheses do not mean five separate investigations. Rule them out starting with what is easy to measure. Temperature and humidity in storage and the work records either exist already or can be gathered in a few days, and thickness can be read at once with a gauge. The ingredients are a matter of opening the TDS and SDS. Scraping under the film and comparing test panels come after that.

The first clue is the shape of the rust. Pinpoint spots spread evenly over flat faces point to gaps in the film, while rust following thread crests and edges, where film thins easily, points to film thickness. Rust gathered at film edges, scratches and joints with other metals, with white powder and pits on aluminium, points to galvanic attack driven by graphite. Rust that has crept under the film and lifted it points to pretreatment.

The next clue is when and where. If the same part rusts only in the rainy season or straight after winter deliveries, or only in the top layer or in boxes near walls, look at damp and condensation first. If rust rose only in lots made after a change of subcontractor or formulation, look at pretreatment and the film formulation; if only parts sent to coastal sites or places using de-icing salt rusted, look at chlorides and graphite together.

If that still does not settle it, run control trials. Make identical steel panels split by pretreatment or none, graphite or graphite-free formulation, and specified or thin film, change only one thing at a time, and put them in the same salt spray cabinet or the same store. Use the results to rank, not to read off field life directly. After the fix, count rust cases on the same basis in the season and place where rust appeared and compare with before; the job is done only when that number falls.

The hypotheses can overlap. A thin film lets water in the same way a porous one does, and without pretreatment that water reaches bare metal at once. When condensation meets a graphite film, the water film that completes the cell forms by itself. In such cases, first correct what can be fixed within the process, such as pretreatment and film thickness, then reduce damp in storage, and only then decide on a change of formulation, because while the process is unsettled, the effect of changing formulation cannot be compared fairly.

Limits and cautions

Film thickness, cure conditions, pretreatment methods and required salt spray hours differ by formulation, part and specification, so numeric decisions follow the film's TDS and the applicable specification. The military specification figures here come from that specification's test conditions. Accelerated tests such as salt spray are useful for comparing formulations but do not state field life as it is, and for parts where rust bears on safety, such as aerospace parts, safety fasteners and pressure parts, do not reuse or release them on floor judgement alone; get design and quality engineers to confirm.

Safety matters too. For dry film sprays, thinning solvents and phosphating chemicals, follow the product's SDS for ventilation, protective equipment and control of ignition sources. Guard against dust and noise in blasting, and wear gloves and eye protection when scraping film with a knife or cutting sections. If rust is heavy enough to cast doubt on a part's strength, do not judge by appearance; have it assessed by a laboratory.

Sources

  1. Asbeck, W. K., & Van Loo, M. (1949). Critical pigment volume relationships. Industrial & Engineering Chemistry, 41(7), 1470–1475. https://doi.org/10.1021/ie50475a042
  2. ASTM International. (2019). ASTM B117-19, Standard practice for operating salt spray (fog) apparatus. https://store.astm.org/b0117-19.html
  3. ASTM International. (2022). ASTM D7091-22, Standard practice for nondestructive measurement of dry film thickness of nonmagnetic coatings applied to ferrous metals and nonmagnetic, nonconductive coatings applied to non-ferrous metals. https://store.astm.org/d7091-22.html
  4. ASTM International. (2026). ASTM D2649-26, Standard test method for corrosion characteristics of solid film lubricants. https://store.astm.org/d2649-26.html
  5. Coelho, L. B., Taryba, M., Alves, M., Montemor, M. F., & Olivier, M.-G. (2018). Unveiling the effect of the electrodes area on the corrosion mechanism of a graphite - AA2024-T3 galvanic couple by localised electrochemistry. Electrochimica Acta, 277, 9–19. https://doi.org/10.1016/j.electacta.2018.04.187
  6. Gresham, R. M. (2003, October). Solid film lubricants: Unique products for unique lubrication. Tribology & Lubrication Technology, 28–31. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Friction/Solid%20Film%20Lubricants_Unique%20Products%20for%20Unique%20Lubrication_tlt%20article_Oct03.pdf
  7. Hihara, L. H., & Latanision, R. M. (1992). Galvanic corrosion of aluminum-matrix composites. Corrosion, 48(7), 546–552. https://doi.org/10.5006/1.3315972
  8. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  9. International Organization for Standardization [ISO]. (2017). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application. https://www.iso.org/standard/58061.html
  10. Narayanan, T. S. N. S. (2005). Surface pretreatment by phosphate conversion coatings – A review. Reviews on Advanced Materials Science, 9, 130–177. https://eprints.nmlindia.org/337/
  11. Peterson, M. B., & Johnson, R. L. (1953). Friction and wear investigation of molybdenum disulfide: I. Effect of moisture (NACA Technical Note 3055). National Advisory Committee for Aeronautics. https://ntrs.nasa.gov/citations/19930083561
  12. Sangaj, N. S., & Malshe, V. C. (2004). Permeability of polymers in protective organic coatings. Progress in Organic Coatings, 50(1), 28–39. https://doi.org/10.1016/j.porgcoat.2003.09.015
  13. U.S. Department of Defense [DoD]. (2013). MIL-PRF-46010H, Performance specification: Lubricant, solid film, heat cured, corrosion inhibiting. https://everyspec.com/MIL-PRF/MIL-PRF-030000-79999/MIL-PRF-46010H_52119/
  14. Vernon, W. H. J. (1935). A laboratory study of the atmospheric corrosion of metals. Part II.—Iron: The primary oxide film. Part III.—The secondary product or rust. Transactions of the Faraday Society, 31, 1668–1700. https://doi.org/10.1039/TF9353101668

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.