KALTECKOREA

BlogApplication notes

Why do threads and fits bind after dry-film coating?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Specialty Tribology

Rubbing the film off or re-tapping the thread is the usual response when coated threads or pins bind, but that only strips film from where it belongs, and whatever made it build up stays for the next lot. What actually lies behind it can be film that is too thick, uneven spraying, film pooled in thread roots and corners, film that sagged, or missed masking, and sometimes two or more at once.

Background

A coated bolt fresh from the oven is being run into a nut on the assembly line, and after two or three turns it stops. At the next station a coated pin catches at the mouth of its hole and the operator reaches for a mallet. Forcing it scrapes the film off, so lubrication and rust protection are lost at that very spot, and parts that still will not go in have to be stripped and recoated or scrapped. When a whole lot binds the line stops, and when only some parts bind they have to be sorted out.

A resin-bonded dry film mixes a lubricating pigment with a binder, solvent and additives; it is sprayed or dipped like a paint and then baked to cure. Threaded fasteners are the largest single use of such films, and unlike paint, the thickness suited to lubrication and wear is very thin, around 5 to 13 µm (Gresham, 2003). The military specification for heat-cured films likewise holds the average thickness to 0.008 to 0.013 mm with every reading between 0.005 and 0.018 mm, and notes that because the cured film is relatively soft, its thickness must be considered on small parts that run with very little clearance. Where it causes interference, the film wears away rapidly until the interference is gone (DoD, 2013).

On threads even a film this thin counts. Film on a flank of a 60-degree thread, the sloping face of the thread, has to be divided by the sine of the 30-degree half-angle and doubled for the diameter, so the pitch diameter grows by four times the film thickness. Class 2A is the external thread class that carries an allowance for plating; class 3A external threads and internal threads have none (NBS, 1969). Metric threads likewise separate the g position, set back slightly from basic size, from the h position, which has no such set-back (ISO, 2013), and the fastener standards for electroplated and zinc flake coatings each give an annex to coating thickness and thread clearance (ISO, 2018; ISO, 2022).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: set aside a few parts that bind and a few that fit, log the film thickness and thread gauge results for that lot, and compare the thickness, application and cure conditions in the film's technical data sheet, the TDS, and in the work instruction with the actual conditions on the day.

Hypothesis 1: film too thick

Film that is thick all over usually comes from how the work is done: spraying heavily to save passes, adding one more pass where the coat looks thin, recoating worn parts straight over the old film, or judging thickness by colour and sheen instead of measuring it. Think of parts back for repair. They were sprayed once more over the old film and baked, and while nuts run all the way onto new parts, they stop halfway on the recoated ones.

A film on a thread grows the diameter by four times its thickness, not once, because the flanks are inclined. The 2A allowance is regarded as adequate for coatings up to about one sixth of that allowance, a figure that already reckons with uneven thickness and symmetry in real coating. Where more coating is needed, the advice is to reduce the maximum thread limits before coating by six times the minimum coating thickness and the minimum limits by four times (NBS, 1969). So a film that fitted within the allowance when first applied can exceed it once another layer goes over the old one. The excess film is the softer side and shears away as the part goes in, but resistance rises while it does and the film left at that spot is thinner (DoD, 2013).

Checking starts with thickness. A gauge probe cannot sit on a thread flank, so measure a flat panel coated alongside under the same conditions, or a flat area on the part, with a non-destructive gauge. Standard practice covers magnetic gauges for non-magnetic films on steel and eddy-current gauges for films on non-ferrous metals (ASTM International, 2022). Check the threads after coating with a GO ring or plug gauge to see whether it runs fully on (ISO, 1996), and compare the gauge result for the same part before and after coating. Results on panels do not always match those on the real part, so the specification advises testing thickness and adhesion on actual parts where possible (DoD, 2013).

If the thickness is out of range, change the recoating rule first. Strip the old film from parts to be recoated and start again from bare metal, and write the number of passes and the target thickness into the work instruction to match the TDS range. Keep the panel thickness and thread gauge result for each lot, so that a rising trend is caught before parts start to bind. Where film is needed on threads with no allowance, such as class 3A or internal threads, agree pre-coating size reductions with the design side.

Hypothesis 2: uneven spraying

When the average thickness is right but it varies from part to part, or from face to face on one part, suspect the way it is sprayed. It happens when gun distance, the air pressure that shapes the fan, or the overlap between passes differs between operators, when small parts in a basket are sprayed from one side only, or when round parts are sprayed without turning them. Take a day when two people sprayed the same pins from the same instruction. One operator's pins are an even matt finish, while the other's shine on the one face that faced the gun, and that face catches first when the pin goes into its hole.

Where sprayed coating lands, and how much, is decided by the gun set-up and the shape of the part together. A study of an air spray gun by simulation and experiment reported that the fan-shaping air pressure and the target geometry strongly affect film thickness distribution. At lower shaping air pressure the coating was concentrated in the centre, while raising it stretched the fan in one direction, narrowed it in the other and spread it over a larger area; spraying tests on a flat plate, a tilted plate and a cylinder confirmed the model (Xie & Wang, 2019). Pass a centre-heavy fan without overlap and thick and thin stripes alternate, and the side of a round part facing away from the gun gets less film. The application method for dry films is chosen by the number and size of parts, thickness, tolerance, and masking and overspray allowances, and spraying in several thin coats generally gives the best lubrication (Gresham, 2003).

To check, measure one part at several points. Measure round parts at four positions around the circumference, and measure parts sprayed in a basket separately according to whether they lay on top or underneath. Compare against the records whether the thickness differences follow the operator, the gun or the shift, and spray one stationary burst onto a blank panel to see the width of the fan and the pattern at its centre. If the tight face is always the face that was towards the gun, this hypothesis is the strong candidate.

If spraying looks like the cause, turn what is left to the operator's hand into numbers. Write gun distance, shaping air pressure, fluid flow, overlap and the number of passes into the work standard, put round parts on a turntable or fix their angle with a jig, and turn basket parts over for a second pass. Build the film in several thin coats rather than one heavy one, and coat one panel alongside whenever the operator changes, to keep a thickness record.

Hypothesis 3: pooling in roots

When thickness on flat faces is in range but only the threads bind, the film may have pooled in concave places. It shows up on fine-pitch threads, on parts with inside corners such as keyways and shoulders, where dipped parts are not spun or shaken off well, and with coating used thicker than the TDS viscosity. Suppose fine-thread bolts were dipped and hung at an angle to dry. The film on the shank is even, but on the few threads facing downwards the roots look shallow, while the crests show a glint of bare metal.

A wet film redistributes itself according to surface tension and the curvature of the surface. Even with uniform surface tension, places where curvature changes, such as inside and outside corners, sharp edges and holes, set up capillary pressure differences that drive the film to uneven thickness. Liquid gathers and builds up in concave corners, while at a sharp edge the pressure is high, the liquid is driven away and the film becomes very thin, and the displaced liquid piles up below and leaves a run mark (Eley & Schwartz, 2002). A thread root is a concave corner and a crest is a sharp edge, so on a thread the same forces can work towards filling the roots and thinning the crests. When the roots fill, there is less room for the mating thread's crests, and the fit binds.

A magnifier settles much of this hypothesis. Look for roots that appear filled and rounded, for bare metal showing on the crests, and for pooling concentrated on the threads that hung lowest. Note whether a ring gauge catches on the first few threads or is tight evenly all the way. On parts with inside corners, a section cut through the corner shows directly how much film has built up there.

If pooling is the cause, change the process to remove surplus coating before it cures. Shake or spin dipped parts to throw off excess liquid, and blow thread roots out lightly with compressed air. Thin the coating to the viscosity range set by the TDS, and when hanging parts to dry, turn them so the threaded end is not lowest. For parts that pool often, review with the supplier whether several thin sprayed coats would serve better than dipping.

Hypothesis 4: sagged film

On parts hung upright to dry or bake, check whether the film ran before it set. Sagging is likely when the film went on thick in one pass, when parts went straight into the oven without time for the solvent to flash off, or when the coating was thinned beyond the TDS. Hang pins vertically, bake them, and a thick band of film has gathered at the lower end. That end is the first to enter the hole in assembly, and once it is past, the rest of the pin slides in easily.

A wet film on an inclined or vertical face flows downwards under gravity. The gravitational shear stress driving this flow is proportional to the wet film thickness and density, zero at the film's free surface and greatest where the film meets the substrate (Eley & Schwartz, 2002). The thicker the wet film, the greater the force at the substrate, so a heavily applied film runs further before it sets, and the coating that runs collects and cures at the lower end or along an edge. The specification for heat-cured dry films likewise calls for a film free of runs and sags, and has applicators air-dry for at least 30 minutes, or flash for 10 to 30 minutes at 65 to 70°C, to drive the solvent off before baking (DoD, 2013).

Whether it is sagging becomes clear quickly once the build-up is matched against how the parts hung. A thick band or drop that is always at the end that hung lowest means sagging; build-up regardless of orientation points to another hypothesis. Measure the thickness at the top and bottom ends of the same part to record the difference in numbers, and find in the records how long parts stood between coating and the oven, and the coating viscosity at the time.

To prevent sagging, apply thin coats and keep to the drying or flash time the TDS sets between them. Rehang parts so the fitting face is not lowest, or for short parts consider baking them lying flat. Adding a step to the work standard that removes drops from the lower end before the oven is another option. If the records show the coating was thinned beyond the TDS range, correct the thinning ratio first.

Hypothesis 5: missed masking

When the tight spot is a surface that was never meant to be coated, the suspect is masking. This is film getting into places that should stay bare, such as tapped holes, fit bores, bearing seats and datum faces; it happens when the drawing does not make the coating area clear, when masking plugs or caps have been reused until they are loose, or when overspray drifts into a hole. On the day the outer sliding face of a housing was sprayed, one of several tapped holes was missing its plug. On the assembly line the bolts run freely into every other hole, but in that one hole the bolt stops halfway.

Why an unmasked surface causes trouble shows in the dimensions of internal threads. The thread standard makes no provision for relieving internal threads, since coatings on them are not generally required, and notes that it is very difficult to deposit a significant thickness of coating on the flanks of internal threads. Where an internal thread must be coated, it has to be enlarged before coating (NBS, 1969). Film that gets in unplanned therefore eats straight into the fit with no allowance to absorb it, and the same holds for fit bores and bearing seats with very small clearances (DoD, 2013). That is also why masking and overspray allowances are weighed from the outset when choosing how to apply a dry film (Gresham, 2003).

First confirm whether the tight spot is, on the drawing, a coated face or one to be left bare. Look for the colour of the film on faces that should be bare, and compare before and after coating with a GO plug gauge for internal threads and with a plug gauge or bore gauge for fit bores. Check the masking records and the leftover masking materials to see whether the plugs and caps used that day matched the number of holes and whether any were loose or torn.

Once missed masking is found, mark coated and masked faces clearly on the drawing and keep a checklist for each part listing the places to mask and the number of plugs. Replace plugs and caps after a set number of uses, and set the spray direction so the gun does not point into holes. Before cutting film out of an already coated internal thread or bore with a tap or reamer, confirm the film's stripping method, and whether rework is allowed, with the supplier and the quality engineer.

Finding the cause

Most of the five hypotheses can be sorted out with a few samples, gauges and a thickness gauge. Whether the face was meant to be coated, whether the panel coated alongside is in range, and whether the gauge runs fully on can all be seen at once without stopping the line, so start there. Sectioning parts or recoating under changed conditions comes after.

Next is where and how the tightness is concentrated. If the whole lot is evenly tight and the panel is thick too, look at film thickness. If it follows an operator, a gun or one face of the part, suspect the spray set-up; if flat faces are fine but thread roots and inside corners are filled, suspect pooling. A thick band at the end that hung lowest points first to sagging, and trouble in only one hole or one internal thread points to masking.

If that still does not decide it, run control trials that recoat with one change at a time. Split parts from the same lot: on one group reduce only the number of passes, on another change only the hanging direction, and on a third have one operator coat with a fixed gun set-up. Change several conditions at once and there is no telling which one worked. Measure the panels and the real parts by the same method and compare them.

The final check uses both gauges and real assembly. Parts coated under the corrected conditions should pass the GO gauge and run fully into their real mating parts by hand or with the specified tool. Count how many parts in a set quantity bind on the same basis as before the change, and the job is done only when that figure has recovered.

The hypotheses can overlap. The thicker the wet film, the greater the gravitational shear stress at the substrate (Eley & Schwartz, 2002), so a heavily applied film makes sagging worse, and it also leaves more coating to collect in concave places. Uneven spraying thickens one face and leads the same way. In such cases put film thickness and spray set-up right first and then look at pooling and sagging again, because while the thickness is unsettled, the effect of changing hanging direction or viscosity cannot be compared fairly.

Limits and cautions

Suitable film thickness, thinning, and drying and baking conditions differ by film product and substrate, so numeric decisions follow the product's TDS, and thread classes and pre-coating sizes follow the drawing and the design engineer's requirements. For aircraft parts and safety-related joints, do not strip film or re-cut threads on floor judgement alone; follow an approved rework procedure and get the quality engineer's confirmation.

Safety matters too. Handle the solvents and spray mist of dry-film coatings with the ventilation, respiratory protection and gloves set out in the product's safety data sheet, the SDS, and keep sparks and static away. Let parts from the oven cool fully before gauging them, and follow the SDS of any stripping chemical used to remove film.

Sources

  1. ASTM International. (2022). ASTM D7091-22, Standard practice for nondestructive measurement of dry film thickness of nonmagnetic coatings applied to ferrous metals and nonmagnetic, nonconductive coatings applied to non-ferrous metals. https://store.astm.org/d7091-22.html
  2. Eley, R. R., & Schwartz, L. W. (2002). Interaction of rheology, geometry, and process in coating flow. Journal of Coatings Technology, 74(932), 43–53. https://www.paint.org/wp-content/uploads/2021/09/jctSEPT02-Eley.pdf
  3. Gresham, R. M. (2003, October). Solid film lubricants: Unique products for unique lubrication. Tribology & Lubrication Technology, 28–31. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Friction/Solid%20Film%20Lubricants_Unique%20Products%20for%20Unique%20Lubrication_tlt%20article_Oct03.pdf
  4. International Organization for Standardization [ISO]. (1996). ISO 1502:1996, ISO general-purpose metric screw threads — Gauges and gauging. https://www.iso.org/standard/6092.html
  5. International Organization for Standardization [ISO]. (2013). ISO 965-1:2013, ISO general purpose metric screw threads — Tolerances — Part 1: Principles and basic data. https://www.iso.org/standard/57778.html
  6. International Organization for Standardization [ISO]. (2018). ISO 10683:2018, Fasteners — Non-electrolytically applied zinc flake coating systems. https://www.iso.org/standard/70609.html
  7. International Organization for Standardization [ISO]. (2022). ISO 4042:2022, Fasteners — Electroplated coating systems. https://www.iso.org/standard/77913.html
  8. National Bureau of Standards [NBS]. (1969). Screw-thread standards for federal services: Handbook H28 (1969), Part I. U.S. Department of Commerce. https://nvlpubs.nist.gov/nistpubs/Legacy/hb/nbshandbook28-1969p1.pdf
  9. U.S. Department of Defense [DoD]. (2013). MIL-PRF-46010H, Performance specification: Lubricant, solid film, heat cured, corrosion inhibiting. https://everyspec.com/MIL-PRF/MIL-PRF-030000-79999/MIL-PRF-46010H_52119/
  10. Xie, X., & Wang, Y. (2019). Research on distribution properties of coating film thickness from air spraying gun—Based on numerical simulation. Coatings, 9(11), 721. https://doi.org/10.3390/coatings9110721

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.