KALTECKOREA

BlogApplication notes

Why does a dry-film coated slide squeak?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Specialty Tribology

Recoating on the assumption that the film has worn out is the usual response to a squeak, but the sound is a vibration from the surfaces sticking and slipping in turn because friction at rest exceeds friction in motion, so it can occur with film still in place. What actually lies behind it can be the gap between static and kinetic friction, a worn-through film, load outside its range, unsuitable surface roughness, or changes in humidity and temperature, and sometimes two or more at once.

Background

A dry-film coated slide starts to move slowly and gives a high squeak, and when pushed by hand it catches and releases in short jerks instead of gliding. If sound were the only problem it might be tolerable, but this motion upsets stopping positions on equipment that must place things precisely, and on a product in customers' hands it comes back as noise complaints. Motion that sticks and slips in turn can lead beyond noise to energy loss, surface damage and component failure (Berman et al., 1996).

This is called stick-slip. While two surfaces in contact are at rest, static friction holds them together; the moment the pushing force exceeds it, they break free and slide quickly, and while sliding, a smaller kinetic friction slows the motion. Because static friction is usually greater than kinetic friction, the sliding surface sticks again, force builds again, and the cycle repeats. The fine tone of a violin string and the squeak of a door are the same phenomenon (Gresham, 2011). A squeak is this cycle setting the part vibrating and that vibration spreading into the air, and sound from friction is a main subject in the acoustics of friction (Akay, 2002).

A dry film holds lubricating pigments such as molybdenum disulfide, graphite or PTFE in a binder and is used to lower friction on sliding faces that carry no oil. Friction coefficient and response to moisture vary with the pigment-to-binder ratio and the pigment type, so the conditions under which a squeak appears differ from one product to the next even among dry films (Gresham, 2003).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: note at what speed and load, how many hours into running, and in what weather the squeak occurs, and compare that, together with how many strokes the part has made since coating, against the operating range in the film's technical data sheet, the TDS.

Hypothesis 1: high static friction

If the squeak appears only at very low speed and disappears as speed rises, or is worst on the first move after standing for a while, look first at the gap between static and kinetic friction. It shows up readily on equipment with a soft drive train, such as long thin rods, belts or loose mountings, and on positioning devices that push a little and stop over and over. Take an inspection jig left standing overnight and run for the first time in the morning. The slide squeaks for the first few low-speed starts, yet the sound fades when the same slide is run back and forth quickly.

The source of the squeak is static friction that grows while the surfaces are stuck. The longer they stay at rest, the more time static friction has to build, so the slower the motion, the larger each stick and release; as speed rises the amplitude shrinks, and at some speed stick-slip stops (Gresham, 2011). One analysis put this in numbers: stick-slip occurs when static friction initially grows faster than about half the product of sliding speed and the spring constant of the drive, and its amplitude is proportional to the final difference between static and kinetic friction. The same analysis shows that stick-slip stops once sliding speed or spring constant passes a critical value (Gao, 1995). So the squeak is set not by one friction coefficient but by the difference between the two frictions, the sliding speed and the stiffness of the drive acting together. That is also why friction models must weigh speed, temperature and load as well as materials and roughness (Ibrahim, 1994).

Listen while changing speed. Recording the speed below which the squeak starts, and whether the first start is noisier the longer the part has stood, shows whether static friction is behind it. If a force gauge can be fitted, measure the peak force at breakaway and the average force while sliding separately, and keep the results with the test conditions as the standard guide on measuring and reporting friction coefficients advises (ASTM International, 2024). On the drive side, check by hand for loose mounting bolts, belt tension and flex in long linkages.

The remedy is to leave static friction no time to build. Where the equipment allows, move the running speed into the range where the squeak stops, and raise drive stiffness by tightening mountings or making linkages shorter and thicker. If low-speed running is unavoidable, choose with the supplier a formulation with a smaller gap between static and kinetic friction and compare the sound at the same speed.

Hypothesis 2: worn-through film

If a sliding face that was quiet for the first few months starts squeaking one day, the film may have reached its end. Parts with many strokes, parts that shuttle over the same short track, and equipment with no set interval for recoating fall here. Consider the transfer rail on an assembly machine. Quiet until last week, the rail squeaks this week, a band of metallic shine shows through the grey film down the middle of the wear track, and black powder has gathered at its edges.

How a film ends shows up in life tests. In oscillating tests of a bonded molybdenum disulfide film, friction fell little by little as strokes added up and then rose suddenly at one point, and that sudden rise marked the end of life. In the same study, most of the film thickness remained until near the end, and rather than thinning evenly, the film ended by coming away from the substrate under repeated shear stress from friction (Hiraoka, 2022). A study observing burnished molybdenum disulfide films found that in moist air the metallic-coloured film failed by turning into a black powder of iron and molybdenum oxide, while in dry argon it was gradually depleted as it was pushed sideways out of the contact (Fusaro, 1982). Where the film is gone, metal meets metal and friction jumps, so a quiet face can start to squeak.

Wipe the wear track with a dry cloth and look. Check whether metallic shine shows in the middle of the track, whether film edges have lifted and flaked like scales, and whether black powder or red rust dust has gathered. Estimate the strokes made since coating from the machine counter or output and compare with when the same part squeaked before. On equipment that logs friction force, look for a point where friction eased off slowly and then jumped.

If the film has reached its end, recoating from scratch beats patching. Strip the remaining film and powder, go through degreasing, blasting and pretreatment, apply to the TDS thickness and cure under the set conditions. If the same part keeps reaching end of life, set a recoating interval from its stroke count and life test results, and if life falls short, review with the supplier a design that reduces load or sliding distance, or a longer-life formulation.

Hypothesis 3: load out of range

Load is the suspect when the parts carried on a jig have changed, when a spring or clamp force has been reset, or when the same film has started being used on other equipment of very different weight. Load is a problem when it is too heavy and also when it is too light. What if a tray that slid carrying only light plastic covers one day starts carrying thick metal parts? It is quiet for the first few days and then begins to squeak at the same spot, while on another slide from which a heavy tool was removed, every light push now squeaks.

The relationship between load and friction coefficient differs from that in ordinary oil lubrication. Solid lubricants generally show a lower friction coefficient as contact pressure rises (Scharf & Prasad, 2013). In tests on thin sputtered molybdenum disulfide films, the friction coefficient fell as load rose, in proportion to load to the power of about -0.32, which was well explained by the film's shear strength divided by contact pressure (Singer et al., 1990). Put the other way round, a lightly loaded face with low contact pressure has a higher friction coefficient and room for static friction to grow. A heavy load brings the opposite problem. The life of a bonded film is explained by fatigue from shear stress between film and substrate (Hiraoka, 2022), so a heavy load ends the film sooner and leads to the sound of metal on metal.

Begin by measuring the actual load. Weigh the parts and tools carried now, not the drawing value, measure spring and clamp forces, divide by the contact area and compare with the load range stated in the TDS. Check from the shape of the track whether load is skewed so that only one edge of the sliding face is touching. On equipment where load can be varied, step it through several levels to find the range in which the squeak occurs.

Load problems are solved by bringing contact pressure back into the range where the film works well. On a face that is too lightly loaded, raise pressure by reducing contact area or adding a little preload; on one too heavily loaded, enlarge the contact area or share the load. If only one edge touches, correct alignment first. Where the design must move the load range a long way, choose a formulation suited to that range with the supplier again.

Hypothesis 4: surface finish

This hypothesis comes in when the coated part is unchanged but the mating part has been newly machined or ground, when the counterface material or machining method has changed, or when blasting conditions for the surface to be coated have shifted. Counterface roughness bears on both the sound and the film's life. On the day a worn mating block is swapped for a freshly ground one during maintenance, with film and load unchanged, the squeak comes only on the new, mirror-smooth block.

Roughness plays two parts. One is the size of the stick-slip, set at the contact. In the analysis cited earlier, rougher contacts had static friction that initially grew faster but reached a smaller final value over a shorter time, so each stick and release was smaller. The same analysis reports that a thicker liquid film on the surface makes that amplitude larger (Gao, 1995). The other, on the coated side's substrate, is where the film can stay. In a study of molybdenum disulfide films on substrates of different roughness, rougher substrates gave longer life, because valleys held lubricant in reserve and gave wear debris somewhere to settle, and during running-in the peaks were flattened and the film flowed across them (Fusaro, 1982). Solid lubricants lower friction by building a thin transfer film on the counterface and sliding film on film (Scharf & Prasad, 2013), so the coated face and the counterface both need suitable roughness for quiet sliding.

Compare machining records and roughness of the counterface. Measure surface roughness on a mating part that squeaks and one that does not with the same instrument, and search the records for changes in material, heat treatment or machining method. See whether a grey or black transfer film covers the counterface evenly, or whether it is still bare metal. On the coated side, check blasting conditions and substrate roughness against the records. Confirm as well that no oil or washing fluid is left on the counterface.

If the counterface cannot be changed, give the transfer film time to settle through running-in. After fitting a new counterface, run it back and forth for a while at light load and suitable speed to carry film across, then move to normal running. Where counterface machining can be specified, write a roughness range on the drawing based on parts that did not squeak, and match the substrate blasting conditions to it. Remove leftover oil from the counterface by degreasing.

Hypothesis 5: humidity and heat

If the same equipment squeaks only in the rainy season, or only in winter when heating has dried the air, look at moisture. A squeak that comes on the first run in the morning and fades as the machine warms up, or one heard only after the doors were left open overnight, also belongs here. Which way moisture acts is opposite depending on the pigment. On a Monday morning after a week of rain, in a plant left over the weekend with air conditioning off, a slide coated with molybdenum disulfide film squeaks and then quietens after an hour or two of running.

Moisture acts on the two pigments in opposite ways. Early work on molybdenum disulfide found the friction coefficient higher at high humidity, even with thick bonded films where metal-to-metal contact was unlikely. The same report also cites earlier work showing that moisture adsorbed on steel raises the coefficient of static friction (Peterson & Johnson, 1953). In tests on sputtered films, below a transition temperature friction rose with more water, and as temperature rose adsorbed water was driven off and friction fell, with the transition between 100 and 250 °C depending on the film and its history (Khare & Burris, 2013). Machines usually warm to far less than that, so this result alone cannot explain a squeak fading as the machine warms; it only suggests a change in the same direction, with less adsorbed water. Graphite is the opposite and needs moisture to do its job. Its slipperiness comes not from crystal structure alone but from adsorbed vapour films such as water, so in very dry conditions friction and wear can rise sharply (Gresham, 2003; Savage, 1948).

Gather temperature and humidity for the days the squeak occurred. Put a data logger beside the equipment and compare relative humidity, air temperature and machine surface temperature at the time of the squeak with days when it was quiet. Confirming in the TDS and the safety data sheet, the SDS, whether the pigment is molybdenum disulfide or graphite lets that be matched against whether the squeak comes in damp or dry weather. If the squeak fades as the machine warms, note how many minutes after start-up it stops.

If humidity decided the squeak, deal with the air around the machine first. With molybdenum disulfide film, lower humidity by dehumidifying or air conditioning in the rainy season and after weekends, and add a short warm-up run at first start. If a graphite film squeaks in dry winter air, avoid excessive dryness or review with the supplier a change to a formulation with a pigment suited to that environment. Where the machine must work in widely swinging humidity, choose a formulation that has been tested for squeak at both ends of that range.

Finding the cause

There is no need to investigate the five hypotheses one by one in isolation. Rule them out starting with what is easy to measure. The wear track only needs wiping and a look, speed usually just needs a setting changed, and a single data logger gathers temperature and humidity within days. Measuring load or counterface roughness comes after that.

The first clue is the wear track. If metallic shine shows or black powder has gathered, look first at a worn-through film. If the film remains evenly yet the squeak persists, move past film life to causes that can squeak with film in place: the gap between static and kinetic friction, load, the counterface and humidity. A track worn heavily along one edge only means skewed load or misalignment.

The next clue is the conditions under which it squeaks. A squeak only at low speed that vanishes when faster, or worst on the first start after standing, points to static friction and drive stiffness. A squeak that comes and goes with the weather and first start-up points to humidity and temperature; one that began after a change of load carried or a force reset points to load; and one that began after a mating part was replaced points to the counterface. If the face was quiet for a long time after coating and the squeak began suddenly one day rather than gradually, think again of the end of film life.

If that still does not settle it, run control trials that change one thing at a time. Raise speed one step, fit a freshly coated specimen in the same place, swap the mating part for one that was quiet, and change load one step. Change only one thing at a time, or there is no telling which one worked. Afterwards, measure how often it squeaks or how much the stopping position wanders, under the same speed and weather and on the same basis as before, and the job is done only when that figure has recovered.

The hypotheses can overlap. Moist air raises friction on molybdenum disulfide film while opening the path by which the film ends as black powder, and an overly heavy load wears the film quickly and creates metal-to-metal contact. On a thinned film, low-speed running that was fine before shows up as a squeak. In such cases, recoat and correct load and alignment first, then look at humidity and speed, because while the film is nearing its end, the effect of changing other conditions cannot be compared fairly.

Limits and cautions

Permissible load, speed, operating temperature and humidity ranges, film thickness and life differ by formulation, substrate, counterface and type of motion, so numeric decisions follow the film's TDS and the equipment maker's guidance. Research figures cited above come from sputtered films or particular test rigs and cannot be carried straight over to parts in the field. If the squeak comes from safety-related parts such as brakes, steering or safety devices, do not keep them in service on floor judgement alone; get design and quality engineers to confirm.

Safety matters too. For film sprays, thinning solvents and stripping chemicals, follow the product's SDS for ventilation, protective equipment and control of ignition sources. Stop and lock out the equipment before reaching in to inspect a wear track or to change load and speed for a test, and keep clear of pinch points when listening near moving parts. Guard against dust in blasting and film stripping.

Sources

  1. Akay, A. (2002). Acoustics of friction. The Journal of the Acoustical Society of America, 111(4), 1525–1548. https://doi.org/10.1121/1.1456514
  2. ASTM International. (2024). ASTM G115-24, Standard guide for measuring and reporting friction coefficients. https://store.astm.org/g0115-24.html
  3. Berman, A. D., Ducker, W. A., & Israelachvili, J. N. (1996). Origin and characterization of different stick-slip friction mechanisms. Langmuir, 12(19), 4559–4563. https://doi.org/10.1021/la950896z
  4. Fusaro, R. L. (1982). Effect of substrate surface finish on the lubrication and failure mechanisms of molybdenum disulfide films. ASLE Transactions, 25(2), 141–156. https://doi.org/10.1080/05698198208983076
  5. Gao, C. (1995). Stick-slip motion in boundary lubrication. Tribology Transactions, 38(2), 473–477. https://doi.org/10.1080/10402009508983431
  6. Gresham, R. M. (2003, October). Solid film lubricants: Unique products for unique lubrication. Tribology & Lubrication Technology, 28–31. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Friction/Solid%20Film%20Lubricants_Unique%20Products%20for%20Unique%20Lubrication_tlt%20article_Oct03.pdf
  7. Gresham, R. M. (2011, June). Slip-stick: What's it all about? Tribology & Lubrication Technology, 32–33. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Friction/Slip-Stick_What's%20it%20all%20about_tlt%20article_June11.pdf
  8. Hiraoka, N. (2022). Wear life of bonded MoS2 film lubricant. In G. Pintaude, T. Cousseau, & A. Rudawska (Eds.), Tribology of machine elements: Fundamentals and applications. IntechOpen. https://doi.org/10.5772/intechopen.99802
  9. Ibrahim, R. A. (1994). Friction-induced vibration, chatter, squeal, and chaos—Part I: Mechanics of contact and friction. Applied Mechanics Reviews, 47(7), 209–226. https://doi.org/10.1115/1.3111079
  10. Khare, H. S., & Burris, D. L. (2013). The effects of environmental water and oxygen on the temperature-dependent friction of sputtered molybdenum disulfide. Tribology Letters, 52(3), 485–493. https://doi.org/10.1007/s11249-013-0233-8
  11. Peterson, M. B., & Johnson, R. L. (1953). Friction and wear investigation of molybdenum disulfide: I. Effect of moisture (NACA Technical Note 3055). National Advisory Committee for Aeronautics. https://ntrs.nasa.gov/citations/19930083561
  12. Savage, R. H. (1948). Graphite lubrication. Journal of Applied Physics, 19(1), 1–10. https://doi.org/10.1063/1.1697867
  13. Scharf, T. W., & Prasad, S. V. (2013). Solid lubricants: A review. Journal of Materials Science, 48(2), 511–531. https://doi.org/10.1007/s10853-012-7038-2
  14. Singer, I. L., Bolster, R. N., Wegand, J., Fayeulle, S., & Stupp, B. C. (1990). Hertzian stress contribution to low friction behavior of thin MoS2 coatings. Applied Physics Letters, 57(10), 995–997. https://doi.org/10.1063/1.104276

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.