KALTECKOREA

BlogApplication notes

Why is clamp load inconsistent on dry-film coated bolts?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Specialty Tribology

Recalibrating the torque wrench or holding the torque value more tightly is the usual response to scattered clamp load, but how much clamp load a given torque produces is set by friction in the threads and under the head, so as long as friction varies, clamp load varies with it. What actually lies behind it can be uneven film thickness, the temperature and humidity at tightening, film worn by reuse, oil that got in, or incomplete cure, and sometimes two or more at once.

Background

The coated bolts were all tightened to the same value with a calibrated torque wrench, yet when clamp load is measured it differs widely from bolt to bolt. Some work loose under vibration and let the joint open, while others have been pulled far harder than intended, enough to stretch the thread. A joint short of clamp load can leak at the gasket, or leave the bolt carrying the cyclic load in full until it fails in fatigue, while an overloaded bolt can damage its thread at tightening or at the next service.

When clamp load is managed by torque, the wrench sets only the turning effort; how much clamp load that becomes is decided by the friction coefficients between the threads and under the head or nut. The friction coefficient can range from 0.04 to 1.10 depending on materials and lubricants, so torque table values have to be adjusted to the actual friction (Barrett, 1990). That is why the test standard that measures torque and clamp force together derives separate thread, bearing-face and total friction coefficients and a torque coefficient (ISO, 2005).

Real-world scatter is not small either. The spaceflight fastening standard, in the absence of test data, takes torque-controlled preload variation as ±25% for fasteners lubricated at assembly and ±35% for unlubricated ones, and notes that lubricants and coatings can raise preload at a given torque over an unlubricated joint and that the surfaces they are on, or migrate to, also affect it (NASA, 2012). Dry films are widely used on fasteners, threaded fasteners being their largest single commercial use (Gresham, 2003), but the friction of the film itself shifts with how it was made and how it is used, and clamp load shifts with it.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: mark the bolts that came out high and low and keep them apart, log the date and time of tightening, the temperature then, how many times each bolt has been used and the condition of the mating nut, and compare them with the torque and friction conditions in the film's technical data sheet, the TDS, and the tightening instruction.

Hypothesis 1: uneven thickness

There are many ways film thickness can come to differ from bolt to bolt: bolts sprayed from one side in a basket, a few bolts recoated, lots where the operator or the shift changed. Within one bolt, too, the thread and the bearing face under the head can carry different thicknesses. Lay out bolts from the same box and the difference is visible. Some are coated densely right across the bearing face under the head, others have almost no film there, and the clamp load readings broadly fall into two groups as well.

Film thickness changes the friction coefficient itself. A study that tested calcium fluoride, molybdenum disulfide and graphite films about 5 to 20 µm thick concluded that the friction coefficient depends on film thickness, and found that existing adhesion theories of friction did not adequately explain the variation (Whitehouse et al., 1970). Dry films are held to a narrow recommended thickness of around 5 to 13 µm precisely because lubrication and wear performance are best in that range (Gresham, 2003). Thickness enters clamp load another way too. A thread with thick film turns stiffly even before the bolt seats, and the torque spent turning the thread before seating uses up part of the tightening torque without producing clamp load (NASA, 2012).

Check thickness, and check where the tightening torque goes. Measure the bearing face under the head and other flat areas of high-load and low-load bolts with a non-destructive thickness gauge to see whether the two groups differ in thickness (ASTM International, 2022). Recording the turning torque just before seating with a dial torque wrench shows how much torque a thick thread consumes first. To tell whether the thread or the bearing face is responsible, separate thread friction from bearing-face friction in a torque and clamp force test.

Once uneven thickness shows up, even out the application first. For each lot, measure a panel coated alongside and a few bolts and record whether they fall within the TDS range, and decide on the drawing whether the bearing face under the head is coated, applying that the same way to every bolt. For basket spraying, turn the bolts and spray again, and keep recoated bolts separate from the rest. When thickness control is in place, retest the torque and clamp load relationship in that condition and set the torque value from it.

Hypothesis 2: temperature, humidity

If clamp load scatter moves with the season or the time of day, look at temperature and humidity at tightening. Bolts tightened on a winter morning in a poorly heated plant against those tightened in the afternoon, parts brought in from an outdoor yard, and parts tightened while still warm from the oven are such cases. Humid seasons such as the rainy season belong in the picture too. Measure the early-morning and the sunny-afternoon assemblies separately later on, and despite the same wrench and the same torque, the morning group's clamp loads sit to one side.

The friction of molybdenum disulfide films moves less with temperature itself than with the water on the surface, which changes with temperature. In tests on sputtered films, below a transition temperature friction was higher the more water there was, and as temperature rose the adsorbed water left and friction fell, with the transition between 100 and 250°C depending on the film and its history (Khare & Burris, 2013). In powder tests too, the lowest friction came at the highest test temperature, about 150°C, where the harmful effect of moisture was smallest (Peterson & Johnson, 1954). A bonded film likewise showed a friction coefficient of about 0.2 in air and about 0.05 in vacuum, a large difference set by its surroundings (Hiraoka, 2022). Assembly areas run far below these transition temperatures, so what shifts friction at tightening may be the day's humidity and the moisture on the part surface more than temperature itself. When friction changes, so does the clamp load a given torque delivers.

The first step is to record part temperature and room humidity in the tightening log. Plot the clamp load readings against these two values to see whether they lean one way, and run torque and clamp force tests on bolts from the same lot split into a cold group and a group held at room temperature. Clamp load also changes on its own after tightening when temperature changes, through differing thermal expansion of joint and bolt (NASA, 2012), so measure clamp load at the tightening temperature, right after tightening, to compare only the difference in friction.

Where temperature and humidity at tightening divide the clamp loads, bring parts and tools into the assembly area early so they reach its temperature before tightening, and let parts from the oven cool to room temperature first. On sites where conditions swing with the seasons, retest under representative conditions and set the torque value from that. If scatter is still large, controlling clamp load by turn angle or bolt stretch instead of torque can also be considered (NASA, 2012).

Hypothesis 3: worn by reuse

In equipment whose bolts are undone and retightened at every service, bolts reused in final assembly after a trial build, and bolts that live in a jig, suspect film wear. Opening the maintenance records often shows a trend. Clamp load came out even at first assembly, but the more services a bolt has been through, the further its clamp load at the same torque has shifted to one side, and bare metal gleams on part of the thread and under the head of those bolts.

The film slides on the thread and bearing face at every tightening and loosening and is shaved away a little each time. In a study of repeatedly tightened zinc-plated fasteners, the contact surfaces of the thread and the nut face wore significantly, and the friction coefficient changed with that wear (Eccles et al., 2010). In tests that tightened and undid molybdenum disulfide coated bolts three times, preload stayed above that of uncoated bolts, but it began to drop as the cycles went on (Bunting et al., 2016). In wear life tests of bonded films, too, the film held for a period and then fell away suddenly, apparently by de-bonding from the substrate (Hiraoka, 2022).

Begin by knowing how many times each bolt has been used. If there is no record of use, mark the heads, and group the clamp load readings by number of uses. Inspect the thread and the bearing face under the head with a magnifier for thinned film or bare metal, and put new bolts and much-used bolts through torque and clamp force tests under the same conditions to compare friction coefficients. The spaceflight fastening standard likewise has each fastener tightened at least three times in these tests unless reuse is prohibited, so that the change with reuse is built into the scatter (NASA, 2012).

If clamp load shifts with the number of uses, set a reuse limit by testing. Find the number of uses at which clamp load starts to leave the allowed band and replace bolts before that, or reuse only bolts recoated by the specified process. For joints reused often, a separate torque value matched to the friction of used bolts is another option, but only where used and new bolts can be kept from mixing.

Hypothesis 4: oil contamination

This is the case where bolts are meant to be tightened dry on their film, but oil gets in from somewhere. Common routes are nuts and tapped holes that arrive coated in rust preventive, cutting fluid left from an earlier process, assemblers who habitually put a drop of oil on the thread, and greasy gloves. Some lines have nuts that differ box by box. Nuts from one box leave an oily film on the hand while another box is bone dry, and the bolts whose clamp load jumps unusually high were mostly paired with nuts from the oily box.

Oil can act to lower the friction of molybdenum disulfide. In room-air tests, adding 5 to 10% oil to molybdenum disulfide brought friction below that of either molybdenum disulfide alone or oil alone, and the same molybdenum disulfide gave friction coefficients from 0.025 to 0.12 merely by changing how it was applied (Peterson & Johnson, 1954). A bolt with lower friction takes more clamp load at the same torque. This fits the fastening standard's point that lubricants and coatings can raise preload at a given torque and that the surfaces they migrate to affect it as well (NASA, 2012), and when oil reaches only some bolts, those bolts alone jump high and the scatter widens. Nor does oil always help the film: the heat-cured film specification notes that the high fluid pressures in heavily loaded sleeve bearings drastically reduce the wear life of the cured film (DoD, 2013).

Wipe mating nuts and tapped holes with a clean white cloth to see whether oil comes off, and confirm the surface finish of incoming nuts and whether they carry rust preventive from the purchase specification. Whether assemblers apply oil of their own accord is best settled by watching the work. Tighten bolts from one lot into degreased nuts and into oiled nuts and run torque and clamp force tests on each, and the numbers for this site show how far oil shifts clamp load.

If oil proves to be the cause, settle on one lubrication state. Decide whether every bolt is tightened dry on its film or every bolt gets a set amount of a specified lubricant, and set the torque value from torque and clamp force tests in that state. The fastening standard requires those tests to use the same lubricant and the same lubrication process as actual assembly (NASA, 2012). Degrease incoming nuts before use or have them supplied oil-free, and rule out ad hoc oiling on the floor in the work standard.

Hypothesis 5: under-cured film

Look at cure when the oven was overloaded, when large heavy bolts were baked for the same time as small ones, when time was counted from loading rather than from reaching the set temperature, or when temperature varies across the oven. Say a bundle of large flange bolts and some small bolts went into one oven for the same time and came out together. The film on the small bolts is hard, but on the large bolts a fingernail leaves a mark, and a cloth wet with solvent picks up colour when rubbed.

A heat-cured film develops its properties only when its binder has cured at the set temperature for the set time. The specification requires the film to meet every requirement after curing for 1 hour at 204±15°C or 2 hours at 150±15°C, counts cure time from when the part reaches cure temperature rather than from when it first meets heat, and so notes that parts may need to stay in the oven longer than the stated time. It also offers a thermocouple fixed to the coated surface as the way to start timing (DoD, 2013). Large heavy parts heat up more slowly than the oven air, so the film may be under-cured even though the oven log shows the full time. An under-cured film may lack the adhesion and performance the specification requires of a cured one, and such a film may smear or wear differently from bolt to bolt under tightening pressure. The observation that most dry-film failures come from poor pretreatment or other misapplication shows how much weight this process control carries (Gresham, 2003).

Gauge cure first with a solvent rub. Coatings that change chemically as they cure grow more solvent resistant as cure proceeds, so rub with a cloth wet with the specified solvent and compare how much film comes off against a properly cured reference part. Solvent resistance does not prove full cure, however, and the time to reach it also depends on temperature, film thickness and air movement, so judge it together with the oven records (ASTM International, 2019). Fix thermocouples to parts to time when large and small bolts reach cure temperature, and compare the friction coefficients of suspect bolts and of bolts re-baked to specification in torque and clamp force tests.

If the film was short of cure, reset cure time on the basis of part temperature. Bake large heavy parts separately from small ones or leave them longer, and load the oven only so far as air can still circulate. Survey temperatures across the oven at intervals and attach the thermocouple records to the lot record. Decide whether bolts already found under-cured may be re-baked only after confirming with the supplier.

Finding the cause

Several of the five hypotheses narrow sharply just by going through the records. Time and temperature of tightening, the number of uses per bolt and the oven records already exist or can be logged at once, and oil on the nuts and film thickness can be checked with a cloth and a thickness gauge. Time-consuming work such as torque and clamp force testing comes after.

Next, see how the scatter divides. If clamp load splits into two groups by box or lot, suspect film thickness or oil on the nuts, and if only a few bolts jump unusually high, suspect oil first. If it leans one way with time of tightening or season, look at temperature and humidity. If clamp load at the same torque shifts as the number of uses rises, look at worn film, and if it divides by oven batch or bolt size, look at cure.

If that still does not settle it, change one thing at a time in torque and clamp force tests. From one lot, test new against used bolts, degreased against oiled nuts, room-temperature against cold parts, and as-is against re-baked bolts, with only one difference at a time. Deriving thread and bearing-face friction separately also shows whether the trouble lies in the thread or under the head (ISO, 2005).

The final check is the width of the scatter. Measure clamp load on bolts tightened under the corrected conditions by the same method as before the change, and see whether the spread has narrowed. The fastening standard asks for at least six sets of fastening hardware, each tightened at least three times, when establishing preload variation (NASA, 2012), so do not stop after measuring a few. The job is done only when the spread is back within what the joint requires.

The hypotheses can overlap. When oil soaks into a thinned, worn film, wear and oil push clamp load in different directions and the results scatter further, and large, heavy bolts heat slowly and are prone to under-cure. In such cases put the manufacturing conditions such as film thickness and cure right first, and then look at the conditions of use such as temperature, reuse and oil, because while the film itself is unsettled, the effect of changing how it is used cannot be compared fairly.

Limits and cautions

Suitable tightening torque, friction coefficient, film thickness and cure conditions differ by bolt grade, joint design and film product, so numeric decisions follow the product's TDS and the tightening requirements set by the design engineer. For safety-related joints such as pressure vessels, rotating machinery and aircraft, do not change torque values on floor judgement; get the design engineer's approval on the basis of torque and clamp force test data. Measuring clamp load ultrasonically or with load washers gives results that depend on calibration and method, so do it together with the measurement specialist.

Safety matters too. Handle coating materials and degreasing solvents with the ventilation and protective equipment set out in the product's safety data sheet, the SDS. Take care against burns with parts from the oven, and when tightening or loosening at high torque, take a stance and position that will not lead to injury if the wrench slips or the bolt breaks.

Sources

  1. ASTM International. (2019). ASTM D5402-19, Standard practice for assessing the solvent resistance of organic coatings using solvent rubs. https://store.astm.org/d5402-19.html
  2. ASTM International. (2022). ASTM D7091-22, Standard practice for nondestructive measurement of dry film thickness of nonmagnetic coatings applied to ferrous metals and nonmagnetic, nonconductive coatings applied to non-ferrous metals. https://store.astm.org/d7091-22.html
  3. Barrett, R. T. (1990). Fastener design manual (NASA Reference Publication 1228). NASA Lewis Research Center. https://ntrs.nasa.gov/citations/19900009424
  4. Bunting, P., Thompson, V., & Riccardo, V. (2016). Sputtered MoS2 coatings for JET in-vessel fasteners (EUROfusion preprint NJOC-PR(16)15911). Culham Centre for Fusion Energy. https://scipub.euro-fusion.org/wp-content/uploads/eurofusion/NJOCPR16_15911_submitted.pdf
  5. Eccles, W., Sherrington, I., & Arnell, R. D. (2010). Frictional changes during repeated tightening of zinc plated threaded fasteners. Tribology International, 43(4), 700–707. https://doi.org/10.1016/j.triboint.2009.10.010
  6. Gresham, R. M. (2003, October). Solid film lubricants: Unique products for unique lubrication. Tribology & Lubrication Technology, 28–31. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Friction/Solid%20Film%20Lubricants_Unique%20Products%20for%20Unique%20Lubrication_tlt%20article_Oct03.pdf
  7. Hiraoka, N. (2022). Wear life of bonded MoS2 film lubricant. In G. Pintaude, T. Cousseau, & A. Rudawska (Eds.), Tribology of machine elements: Fundamentals and applications. IntechOpen. https://doi.org/10.5772/intechopen.99802
  8. International Organization for Standardization [ISO]. (2005). ISO 16047:2005, Fasteners — Torque/clamp force testing. https://www.iso.org/standard/27788.html
  9. Khare, H. S., & Burris, D. L. (2013). The effects of environmental water and oxygen on the temperature-dependent friction of sputtered molybdenum disulfide. Tribology Letters, 52(3), 485–493. https://doi.org/10.1007/s11249-013-0233-8
  10. National Aeronautics and Space Administration [NASA]. (2012). NASA-STD-5020, Requirements for threaded fastening systems in spaceflight hardware. https://s3vi.ndc.nasa.gov/ssri-kb/static/resources/nasa-std-5020.pdf
  11. Peterson, M. B., & Johnson, R. L. (1954). Friction and wear investigation of molybdenum disulfide: II. Effects of contaminants and method of application (NACA Technical Note 3111). National Advisory Committee for Aeronautics. https://ntrs.nasa.gov/citations/19930083852
  12. U.S. Department of Defense [DoD]. (2013). MIL-PRF-46010H, Performance specification: Lubricant, solid film, heat cured, corrosion inhibiting. https://everyspec.com/MIL-PRF/MIL-PRF-030000-79999/MIL-PRF-46010H_52119/
  13. Whitehouse, G. D., Nandan, D., & Whitehurst, C. A. (1970). The effect of film thickness on friction coefficients for solid lubricants; CaF2, MoS2 and graphite. ASLE Transactions, 13(3), 159–168. https://doi.org/10.1080/05698197008972292

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.