KALTECKOREA

BlogApplication notes

Why does e-coat show gas marks and pinholes?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Coatings & Surface Treatments

Small holes in e-coat are easily taken for dirt or oil contamination and met with more cleaning and degreasing, but gas marks and pinholes can form when gas and electrical discharge inside the film break through it during deposition, so cleaning alone does not remove them. What actually lies behind them can be voltage above the rupture point, gas from zinc-coated steel, a hot bath, too much solvent or high conductivity, and these can act together.

Background

Under a magnifier, a cured part shows small pinpricks scattered across the film, each rimmed like a tiny volcano. On broad faces or edges there may also be patches where the film looks burnt and roughened. Such holes reach the substrate, so at each one the path to corrosion that the primer should block is open (Bubash, 1998). Later coats rarely seal these defects, particularly where the area has been sanded (Schoff, 2016).

In cathodic e-coat the part is the cathode, and water at its surface is electrolysed into hydrogen gas and hydroxide ions. As the pH near the surface rises, positively charged resin particles lose their charge and coagulate into a film (Beck, 1976). As the film grows the current falls, but the film keeps tiny holes where bubbles escaped, and current through the film is carried by ions in those holes. If the voltage is too high, the film cannot grow evenly and breaks down, and the rupture voltage at which it breaks is described as depending on the film's flow properties and the rate of electrolysis (Oyabu et al., 1983). A study that measured film temperature during deposition concluded that film rupture in cathodic e-coat is caused by sparking inside hydrogen bubbles in the film (Doroszkowski & Toynton, 1989).

So the same hole can form in two ways: the current through the film is so strong that discharge and gas burst inside it, or gas formed at the substrate is trapped under the film and blows through it during cure (Bubash, 1998). These holes are often mistaken for dirt or other defects, sending effort to the wrong problem, so a cross-section showing a connected void down to the substrate helps (Schoff, 2016).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: confirm whether the holed parts are cold-rolled steel or hot-dip galvanised, galvannealed or electrogalvanised sheet, and line up the rectifier voltage and ramp time, bath temperature, conductivity, solids and solvent records with the times the defects appeared, comparing them with the paint's technical data sheet, the TDS.

Hypothesis 1: voltage too high

Look at this hypothesis first right after voltage was raised to make film thickness. The same applies when parts of different size and weight share a rack and some draw a concentrated current, when the ramp time for first applying voltage was shortened, when ripple, the pulsation in the rectifier output, has grown, or when parts pass too close to an electrode. Suppose the voltage was raised a step the day after a complaint about thin film. The inner faces now meet the thickness target, but the outer edges facing the electrodes show burnt-looking marks and small holes.

There is a limit to the voltage a film can stand. A troubleshooting source attributes rupture to excessive voltage, excessive ripple, high film build, electrodes too close together and bath contamination, and says parts should be racked by substrate, size and weight so that voltage can be set to suit (Bubash, 1998). High voltage or fast ramps bring bumpy, rough and even ruptured films, and film made thick by high voltage tends to turn bumpy, since e-coat is a primer and not designed for excessive thickness (Tirado, 2017).

How the voltage is applied also changes the outcome. In a study of craters on zinc-rich surfaces, defects fell with lower rectifier ripple, a slower rate of voltage application and greater anode-to-sample distance (Hart, 1985). In experiments that placed a resistance between the power source and the part to soften the abrupt early conditions of deposition, the rupture voltage of phosphated steel rose (Vatistas, 1998). Both results point to the same idea: even at the same final voltage, how abruptly the film grows in the first seconds matters.

The rectifier record is the starting point. Look at voltage, current and ramp time at the times the defects appeared, and measure ripple against the recommendation that it be checked yearly and not exceed 5% under anticipated load (Bubash, 1998). Coat test panels from the same bath at stepwise higher voltages to find where the film starts to rupture, and see how much margin the production voltage leaves. Record also whether holes and burn marks gather near the electrodes or at particular rack positions.

If voltage looks like the cause, the recommended move is to lower it first and make up the lost thickness with other variables such as solids, bath temperature, solvent or dwell time (Tirado, 2013). Ramp more gently, service the rectifier if ripple is high, and rack parts of different size and substrate separately so each gets a suitable voltage. Reset the distance between electrodes and parts to a safe gap as well.

Hypothesis 2: gas from zinc coating

The first question is whether the substrate has changed. This hypothesis moves to the front when zinc-coated parts join a line that ran only cold-rolled steel, when the zinc coating changes to galvannealed, or when a lot arrives whose coating has many fine cracks or pores. Look at a rack carrying cold-rolled steel brackets beside galvanised panels. The brackets are smooth, but the galvanised panels, through the same voltage and the same bath, are scattered with small craters.

Several studies have looked at why zinc makes things worse. A study of craters on zinc-rich surfaces found that susceptibility to the defect is inherent in zinc and explained it as localised dielectric breakdown of the film during deposition. The discharge pushes the paint aside at that spot and cures the surrounding film early, and the cured film does not flow back during baking, so a crater remains (Hart & Townsend, 1983). The study that traced rupture to sparking inside hydrogen bubbles also linked that sparking to the electron work function of the substrate, suggesting that the substrate metal plays a part in rupture (Doroszkowski & Toynton, 1989).

The state of the zinc layer matters too. Voids, micro-cracks or small pores in the zinc layer set up local galvanic cells between the iron base and the zinc, which become the sites where rupture starts, and hot-dip galvanised coatings, with less iron, are in most cases more resistant to rupture than galvannealed ones (Tirado, 2013). When gas formed during deposition is trapped under the film in microvoids of the coating, it blows through the film during cure and leaves volcano-like holes (Bubash, 1998). The electrical discharge that ruptures the film at high voltage is more likely over zinc-coated steels, especially zinc-iron alloys, but can also occur on cold-rolled steel (Schoff, 2016).

Counting by substrate already reveals a lot. Count holes on parts from the same day and the same racks split by substrate and coating type, and by coating lot number where it is recorded. Coating cold-rolled and zinc-coated test panels together in the same bath at stepwise higher voltages shows the difference in the voltage at which each starts to rupture as a number. Comparing the wet film before cure with the cured film also tells holes blown during cure from rupture during deposition.

If defects concentrate on zinc-coated parts, rack them separately with a lower voltage and a gentler ramp. Gassing on galvanised steel depends on the substrate, but changing deposition conditions such as solvent, bath temperature, dwell time and voltage may help (Schoff, 2016), so find the combination on test panels with the paint supplier. If the zinc layer has many voids and pores, ask the coating supplier to improve it.

Hypothesis 3: hot bath

This hypothesis follows the season and the time of day. Bath temperature climbs in summer, when a heat exchanger or chiller loses performance, when a filter on the cooling side clogs, or when long runs let heat from pumping and current build up. On a midsummer afternoon the bath thermometer reads higher than in the morning. Parts from the morning were clean, but pinholes have clearly increased on zinc-coated parts made in the afternoon.

Temperature works in two directions. A warmer bath builds more film at the same voltage, so lowering voltage and making up thickness with temperature is one approach in use (Tirado, 2013). One source even prescribes lowering voltage while raising bath temperature to reduce discharge rupture (Schoff, 2016). A troubleshooting source, on the other hand, names both high bath temperature and high film build as causes of rupture (Bubash, 1998). Which way temperature acts in a given bath therefore has to be settled from the records and on test panels.

Set the bath temperature log beside the defect times. Confirm the thermometer is calibrated against a reference, and measure temperature at several points in the tank and the circulation lines to find any hot spots. Check that the heat exchanger is working from the temperature differences of coolant and paint across it. Coating test panels from the same bath sample at different temperatures and measuring how far the rupture onset voltage moves with temperature makes the judgement clear.

When the evidence leans towards temperature, restore cooling first. Clean the heat exchanger and coolant filters, set the flow and bring the bath back within the TDS range. A cooler bath may give thinner film, so agree with the paint supplier to make up thickness with dwell time or solids rather than by raising voltage.

Hypothesis 4: high solvent

Look at this hypothesis when solvent was added to improve flow, or has been added without a set rule. Lines that draw off very little ultrafiltrate, leaving solvent few ways out, belong here too. A week with solvent additions logged one after another is an example. Film builds thicker than usual and gloss has risen, and from that same week pinholes on zinc-coated parts have increased as well.

Solvent is the component that softens the film and helps it flow. High solvent gives thicker film and higher gloss but lowers rupture voltage and throwing power, and high solvent levels are attributed to excessive solvent additions. Low solvent, conversely, gives thinner film and a higher rupture voltage but poorer flow, which can leave an orange-peel surface (Bubash, 1998). Set beside the description of rupture voltage as depending on the film's flow properties (Oyabu et al., 1983), the softer solvent makes the film, the lower the voltage it can stand. Another source, though, prescribes adding solvent to reduce discharge rupture (Schoff, 2016), so whether solvent is too high or too low is decided by measurement.

Solvent content cannot be seen, so it has to be measured. Analyse a bath sample by the method the paint supplier specifies, often gas chromatography, compare with the TDS range, and review solvent additions and ultrafiltrate draw-off together. Whether a period when film thickness and gloss rose together matches the period when pinholes increased is a useful clue. Measure the rupture onset voltage on test panels and check whether it has dropped below earlier records.

If solvent proves high, stop solvent additions and lower it by drawing off ultrafiltrate in a planned way. Drawing off too much leaves solvent short and flow poor, so set the amount and pace with the paint supplier while watching the measurements. From then on, add solvent only against measured values.

Hypothesis 5: high conductivity

Conductivity tends to creep up rather than jump overnight, so defects often increase gradually too. Typical times are when pretreatment chemicals are carried over on the parts, when deionised water quality has dropped, when anolyte control has slipped, or when solids are high. Take the records for a week when resin regeneration of the deionised water unit ran late. Bath conductivity rises a little each day while the voltage setting stays the same, and from late in the week rupture marks begin to appear.

Ions carry current along fine paths through the film. Film conduction depends on ions in the holes left by escaping bubbles, and ions brought in from earlier stages accumulate in the bath and degrade deposition efficiency and film appearance (Oyabu et al., 1983). More ions in the bath tend to mean more current through the film at the same voltage, and a troubleshooting source states that high conductivity can bring rupture, high film build and roughness. According to the same source, conductivity rises with high solids and with ionic contamination carried in on parts or by poor deionised water (Bubash, 1998).

E-coat bath conductivity has a defined test method, so measure it that way and plot the trend (ASTM International, 2023b). Measure the conductivity of the deionised water and the rinse just before e-coat as well (ASTM International, 2023a), and see whether the rise in bath conductivity coincides with poorer water quality. Put anolyte conductivity and circulation and the solids readings on the same chart.

If conductivity is high, close the way in first. Put right the rinses after pretreatment and the deionised water unit, and manage the anolyte to the TDS. Ions already in the bath can be brought down by drawing off ultrafiltrate and replacing it with deionised water (Bubash, 1998). Solvent and solids move along with it, so proceed in small steps while measuring.

Finding the cause

Four of the five hypotheses are values already in the records. Rectifier voltage and ramp, bath temperature, solvent additions and conductivity only need setting beside the defect times, so start there. Checking the substrate takes one look along the racks, and rupture voltage measurements on test panels come after that.

Where the defects appear is a strong clue. If only zinc-coated parts are affected and cold-rolled steel is clean, look first at gas from the coated substrate; if they cluster with burn marks near the electrodes or at certain rack positions, look first at voltage and ripple. A rise in the afternoon or in summer points to bath temperature, a rise along with film thickness and gloss after solvent additions points to solvent, and a gradual rise over weeks alongside rising conductivity records points to ionic contamination.

Look at the shape of the holes as well. Gas holes are described as small volcano-like holes with a raised rim that penetrate to the substrate (Bubash, 1998). If they could be confused with craters from oil contamination, cut a cross-section and look for a void running from the substrate to the surface. If the holes already show in the wet film before cure, suspect rupture during deposition first; if they appear only after cure, suspect gas escaping during baking.

If that still does not settle it, change one thing at a time on test panels. Coat cold-rolled and zinc-coated panels together under the same conditions, and with the same bath sample change only temperature or only ramp time while measuring the rupture onset voltage. Testing a production bath sample beside fresh paint separates the bath's solvent and ions from the operating conditions. After each countermeasure, count holes per set area on the same substrate and rack positions and compare with before; the job is done only when that count has recovered.

The hypotheses interlock. High bath temperature, high solvent and high conductivity are all named as causes of rupture, and solvent and conductivity raise film build as well (Bubash, 1998), so when they rise together the margin before rupture at the same voltage shrinks on several fronts. Zinc-coated substrates start with a narrower margin. The safer order is therefore to bring bath conditions back within the TDS ranges first, measure rupture voltage again on test panels for each substrate, and then set voltage and ramp to match.

Limits and cautions

Suitable voltage, ramp time, bath temperature, solvent, solids and conductivity differ by paint, substrate and equipment, so numeric decisions follow the paint's TDS and the supplier's guidance. Judging pores and cracks in the zinc layer and cross-section analysis are work for a laboratory and the coating supplier, and for parts where corrosion resistance matters, do not release on appearance alone; decide with the quality engineer against the customer's criteria.

E-coat equipment carries a high DC voltage, so leave ripple measurement and electrode checks to a qualified electrician, and work in the tank only after the rectifier is switched off and locked out. Run rupture voltage tests on panels in laboratory equipment, not in the production tank. For paint, solvent and ultrafiltrate, follow the product's safety data sheet, the SDS, for protective equipment and ventilation.

Sources

  1. ASTM International. (2023a). ASTM D1125-23, Standard test methods for electrical conductivity and resistivity of water. https://store.astm.org/d1125-23.html
  2. ASTM International. (2023b). ASTM D4399-05(2023), Standard test method for measuring electrical conductivity of electrocoat baths. https://doi.org/10.1520/D4399-05R23
  3. Beck, F. (1976). Fundamental aspects of electrodeposition of paint. Progress in Organic Coatings, 4(1), 1–60. https://doi.org/10.1016/0300-9440(76)80001-X
  4. Bubash, K. (1998, July 1). Troubleshooting for electrocoating. Products Finishing. https://www.pfonline.com/articles/troubleshooting-for-electrocoating
  5. Doroszkowski, A., & Toynton, M. A. (1989). Temperature rise, sparking and film rupture in cathodic electroprimers. Progress in Organic Coatings, 17(2), 191–205. https://doi.org/10.1016/0033-0655(89)80023-8
  6. Hart, R. G. (1985). Factors influencing cathodic e-coat primer cratering on zinc-rich surfaces (SAE Technical Paper 850237). SAE International. https://doi.org/10.4271/850237
  7. Hart, R. G., & Townsend, H. E. (1983). Mechanism of cathodic electrocoat primer cratering (SAE Technical Paper 831818). SAE International. https://doi.org/10.4271/831818
  8. Oyabu, Y., Furuno, N., Hirasawa, Y., & Omori, H. (1983). Electrodeposition coating process for automobile bodies. Transactions of the Iron and Steel Institute of Japan, 23(11), 994–1008. https://doi.org/10.2355/isijinternational1966.23.994
  9. Schoff, C. K. (2016, April). Automotive coatings application defects. CoatingsTech, 32–39. https://www.paint.org/wp-content/uploads/2021/09/Automotive-Coatings-Application-Defects_Apr-2016.pdf
  10. Tirado, J. (2013, December 4). Eliminating voltage rupture. Products Finishing. https://www.pfonline.com/articles/eliminating-voltage-rupture
  11. Tirado, J. (2017, March 1). How to identify and control poor ecoat film appearance. Products Finishing. https://www.pfonline.com/articles/how-to-identify-and-control-poor-ecoat-film-appearance
  12. Vatistas, N. (1998). A new electrocoating technique to avoid cratering and increase voltage rupture. Progress in Organic Coatings, 33(1), 14–19. https://doi.org/10.1016/S0300-9440(97)00114-8

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.