KALTECKOREA

BlogApplication notes

Why does coated steel rust first at edges and welds?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Coatings & Surface Treatments

Rust at edges and welds is easily put down to a weak paint, since they got the same paint and the same number of coats as the flat areas, but wet paint pulls back from sharp edges and cures thin, and welds are uneven before any paint goes on, so the same work does not give the same protection. What actually lies behind it can be thin film at edges, edges left sharp, welds left undressed, a missing stripe coat or salt left at welds, and sometimes two or more at once.

Background

Inspect steelwork, tank interiors or equipment bases a few years after painting, and the flat areas are often still sound while rust has come up in a thin line along flange tips and runs along weld lines in a string of spots. Because edges and welds fail while the flat areas hold, repair painting is needed long before the whole structure is due for repainting, and at height or inside a tank the scaffolding and ventilation can cost more than the repair itself. Left alone, the rust eats away first at the thin section of the edges.

The field record bears this out. In a study of inspection pictures from an offshore platform, a ship's ballast water tank system and two coastal road bridges, corrosion on coated steel mainly began at edges and welds, which accounted for 50% to 90% of the attacks depending on the structure. The same study traced this to low film thickness: wet paint retracts from sharp edges, so the cured film has reduced barrier properties (Knudsen et al., 2023).

Paint protects steel as a barrier that slows water, oxygen and ions on their way to the steel, so wherever the film is thin, protection is weaker by that much (Sørensen et al., 2009). Edges and welds have shapes on which paint readily thins, and welds may carry spatter, slag, pores and residues before any paint goes on. So even with the same paint and the same number of coats as the flat areas, these two places do not get the same protection.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: mark on the drawings whether the rust is at edges or welds, and which edges and which welds, then compare the painting specification, the paint's TDS and the application records for edge treatment, weld preparation, stripe coating and film thickness.

Hypothesis 1: thin film at edges

If rust appears along edges even though they were ground round, first suspect how much paint actually stayed on them. Edge film tends to end up thinner than on flat areas with paints that flow well, with heavily thinned paint, with paint applied thick in one pass that flows a lot while curing, and when spray angle and distance were set for the flat faces. On one side of the shop hang angles and flat bars just painted. The flat faces have an even gloss and the gauge readings meet the specification. Look closely along an edge and the colour is paler than on the faces, and here and there the grain of the metal shows through.

Until it cures, wet paint is subject to surface tension. Surface tension is the force that tries to shrink a liquid's surface, and it pulls paint lying over a convex edge towards the flat faces on either side. So an edge that looked evenly covered just after painting thins as the paint draws back during cure. The field analysis cited above explained edge corrosion by exactly this (Knudsen et al., 2023). With thin film left on the edge, water and oxygen have a short path to the steel, and that is where the coating breaks through first. Tests also show that the degree of rounding alone does not decide the outcome. In a wave chamber simulating a ballast tank, edge radius had no statistically significant effect on the protective performance of the coatings, while the tool and method used to round the edges and the position of the specimen in the chamber mattered more (Momber et al., 2017).

Edge film shows itself as soon as an edge is cut. The gauge probe is designed to sit on a flat surface and does not capture thickness at the very tip of an edge, so grind a cross-section of an edge on a test piece painted under the same conditions, or on a part that can be cut, and compare film thickness on the face and at the edge tip under a magnifier or microscope. On parts in service, record the thickness on the face right next to the edge and whether the substrate shows through anywhere along it. Measure flat-area thickness by the standard for rough surfaces (ISO, 2012).

If the section shows edge film clearly thinner than on the face, adjust both paint and method. Bring thinning and the thickness applied per pass back within the TDS, make a separate spray pass along the edges, and add a step that covers the edges again with the next coat. When changing paint, ask the supplier for edge coverage data, and decide only after comparing actual edge film by the same cross-section check.

Hypothesis 2: edges left sharp

This covers sheet edges cut by gas or plasma, burrs left on sheared edges, the rims of punched holes and as-rolled square corners that were painted untouched. It is easily missed on small parts under delivery pressure, on subcontracted parts, and on parts cut or drilled just before painting. Say a bracket that had a few extra holes drilled went straight onto the painting line. Its outer edges were ground round, but sharp burrs still stand around the new holes and still catch the fingertip after painting.

The shape of an edge decides where paint can stay. A sharp edge or the tip of a burr has almost no radius, so when paint draws back, almost nothing remains at the tip. That is why painting standards and rules require edges to be treated before painting. The design standard for painting steel structures gives guidance on shaping edges and welds so that surface preparation and painting can be done properly, and the standard on preparation grades for welds and edges grades how much work each type of imperfection needs (ISO, 2006, 2017). The coating performance standard for ship ballast tanks requires edges to be rounded to a radius of at least 2 mm, or given three-pass grinding or an equivalent treatment, before painting (IMO, 2006). Given the test result that the tool and method of rounding mattered more than the radius itself, the treatment method should be specified as well as the figure (Momber et al., 2017).

Put a gauge to it. Measure the radius of rusted and unrusted edges with a radius gauge, and draw a fingertip or a cotton glove along the edge to feel for burrs. Mark on the drawings whether rust clusters on cut edges, around punched holes or where machining was done later, and check whether an edge treatment record exists for that part. If the pre-painting checklist has no edge item, that in itself is a clue.

The fix is to treat edges before painting. Write the edge requirement into the specification as a radius or a preparation grade, and state the tool and the number of grinding passes too. For subcontracted parts and parts machined just before painting, add a step in the pre-painting inspection that checks edges separately. On edges that have already rusted, remove the rust and lifted paint, grind the edge round, and repaint.

Hypothesis 3: welds left undressed

This hypothesis gains weight on fabrications with a lot of manual welding, on parts only blasted without grinding after welding, and on site welds that were only brushed before painting. Spatter, small metal droplets thrown around the weld, slag, the glassy residue covering the bead, undercut, the groove melted at the weld toe, and porosity, small holes in the bead surface, all stay under the paint. Here is a tank interior on inspection day. Rust spots line the weld seams, and up close each has a small bead rising at its centre, while in places rust streaks have run down from a fine groove beside the weld.

Beneath a spatter droplet is a place paint cannot reach. A narrow crevice forms at the neck where the round droplet joins the plate, paint draws back from its crown as from a sharp edge, and if the droplet later falls off, bare steel is left behind. Slag is not a layer firmly bonded to the steel, so it can come away together with the paint on it, and undercut and pores leave air pockets the paint does not fill and thin film around them. That is why the ballast tank coating standard requires the surface to be prepared by grinding weld beads and removing spatter and other contaminants, so that the coating covers evenly and adheres well (IMO, 2006). Different imperfections also need different treatment. In a cyclic accelerated test simulating a marine environment, weld ripple and undercut needed only the less thorough preparation grade when a stripe coat was applied, whereas porosity required the higher grade, at which the stripe coat could be left out (Marquardt et al., 2025).

Start from the centre of the rust spots. A bead at the centre points to spatter, rust running along a fine groove beside the bead points to undercut, and pinpoints of rust set in the bead surface point to porosity. On welds not yet painted, count what remains by imperfection type as the preparation grade standard lists them, and compare with the grade the specification requires (ISO, 2006). On painted welds, strip a little paint at suspect spots and check beneath it.

If the evidence leans towards weld imperfections, put a dressing step between welding and painting. Scrape or grind off spatter, remove slag completely, and grind sharp bead toes and undercut into a smooth transition. Write into the specification that porous welds get the higher preparation grade, and decide the grade together with whether a stripe coat will be applied. Setting welding conditions that produce less spatter also cuts the work on the painting side.

Hypothesis 4: no stripe coat

Look at this hypothesis when a tight schedule led to skipping the brushed extra coat, or when the specification did include a stripe coat but did not make clear at which coat or over what extent it applies. It is especially easy to drop on lines that spray large areas quickly, inside tanks and on complex structures that are hard to reach. On one structure, one zone shows a distinct brushed extra coat along edges and weld seams, while the neighbouring zone shows only an even spray pattern. On inspection, the lines of rust are far more frequent on the edges of the neighbouring zone.

The job of a stripe coat is to put an extra, separate layer of paint where film tends to thin. The ballast tank coating standard defines it as painting edges, welds and hard-to-reach areas to secure adhesion and film thickness in critical spots, and requires at least two stripe coats and two spray coats. The same standard has stripe coats applied by brush or roller, with roller only for places such as scallops and rat holes (IMO, 2006). Brushing can work paint into the crevice at the neck of spatter, the undulations of the bead and the very tip of an edge, whereas spray tends to skip such spots or leave them thin. In the weld test described above, too, a stripe coat lowered the preparation grade needed for ripple and undercut (Marquardt et al., 2025).

Records come first. See whether the painting log and inspection sheets show how many stripe coats went on, at which coat and with what tool, and compare that with the number in the specification. On site, check edges and weld seams for brush marks and, if coats were tinted differently, for the colour of the stripe coat. Where a section can be ground, count whether edges and welds carry more coats than the flat areas.

If the stripe coat was skipped or done half-heartedly, make the step explicit in the specification. State before or after which coat it goes on, over what features, and that it is brushed, and tint successive coats differently so that inspectors can check by eye. Add a sign-off box on the inspection sheet so the step is not dropped under schedule pressure. Where rust has already appeared, remove it, dress the edges and welds, and include a stripe coat in the repair painting as well.

Hypothesis 5: salt left at welds

Weigh up salt when welding with flux was followed only by dry blasting or tool cleaning before painting, or when welded parts sat for a while near the sea or in damp conditions before painting. Small blisters rising along the weld seam together with rust spots add weight to this hypothesis. At an outdoor yard of a coastal plant, welded blocks wait several weeks for painting. After blasting, the welds looked the same grey as the rest, and spatter had been ground off cleanly. About six months later, small blisters rise in a row along the weld seams only.

The area around a weld is a different surface from the rest before any paint goes on. The surface cleanliness standard notes that foreign matter can include water-soluble salts and welding residues, and that these may not be fully removed by dry blast cleaning or hand and power tool cleaning, so wet blast cleaning can be used (ISO, 2007). When such salts remain under the paint, water passing through the film gathers there by osmosis and raises blisters, and the concentrated brine inside speeds corrosion (Morcillo, 2003). Not every welding residue is equally harmful. In a test where steel contaminated with welding fume was treated by light to heavy sweep blasting and then coated with epoxy, the remaining fume did not affect adhesion, blistering or cathodic disbondment performance (Shon, 2011). So a weld is not a worry in itself; whether water-soluble salt remains has to be measured.

Take salt samples from the weld and from the flat area beside it. After blasting and before painting, dissolve the salt from the same area at each spot with water, measure the electrical conductivity of that water, and compare the two values. This field conductivity method is set out in a standard (ISO, 2020). Where paint is already on, measure the same way on the surface exposed by stripping paint along a blistered seam, and find in the records where and for how long the part stood between welding and painting.

If welds show high salt, remove it before painting by washing with clean water or by wet blasting, measure again to confirm it is within the limit, and then paint. The ballast tank coating standard sets the water-soluble salt limit for primary surface preparation at 50 mg/m² expressed as sodium chloride, which is a useful reference when setting a specification (IMO, 2006). The actual allowable value follows the painting specification and the paint supplier's guidance; shorten the time between welding and painting, and keep parts covered in the meantime.

Finding the cause

Rule out the five hypotheses starting with what can be seen and felt. Edge radius and burrs, leftover spatter and slag, and the brush marks of a stripe coat can be checked without breaking the paint, and edge treatment and stripe coating also appear in the records. Edge film thickness needs a ground cross-section, and salt at welds can only be measured once paint is stripped, so they come next.

The pattern of the rust points to the cause. Rust running in a long thin line along edges points to edge film, edge treatment and stripe coating, and if it clusters on cut edges and around holes drilled later, to edges left sharp. A bead at the centre of rust spots on a weld, or rust along a groove beside the bead, points first to spatter and undercut; blisters lined up along the seam point first to salt left at welds. If rust lines appear evenly even though the edges were ground round, check by cross-section whether the paint drew back from the edge and cured thin.

If that still does not settle it, compare with test pieces. From the same steel, make pieces that differ in one thing only, such as edges left as cut versus ground by the set method, or with and without a stripe coat, and paint them with the same paint, by the same person, under the same conditions. Grind sections from half to measure film at edges and welds, and hang the rest side by side to see the order in which rust appears. Change only one thing at a time, or there is no telling which made the difference.

The final check comes with the next painting job. Inspect parts painted with the changed process in the same way, and compare when rust first appears at edges and welds, and how many spots, against earlier parts on the same basis. If flat areas, edges and welds now deteriorate at a similar rate, the cause has been caught.

The hypotheses can overlap. A sharp edge is where paint draws back most easily, and if the stripe coat is missing, nothing covers it again; a weld that was only brushed before painting can keep both spatter and salt. In such cases, correct first what can only be fixed before painting. Edge treatment, weld dressing and salt removal cannot be fixed without stripping once paint is on, whereas a stripe coat and edge film thickness can still be added during repair painting.

Limits and cautions

Edge radius, weld preparation grade, number of stripe coats, film thickness and allowable salt level vary with environment, structure and paint, so numeric decisions follow the painting specification, the TDS of the paint and the rules that apply to the structure. Figures in the ballast tank standard are for that use and are not carried over to other structures as they stand. If cracks or large defects in welds are suspected, that is a weld quality matter rather than a painting one; pass it to the weld inspector.

Safety matters too. Grinding and blasting produce dust, noise and flying fragments, so use eye protection, hearing protection and respiratory protection, and for paints and thinners follow the product SDS for ventilation and protective equipment. In confined spaces such as tank interiors follow the set entry procedure and gas testing, and check old coatings for hazardous ingredients before stripping them.

Sources

  1. International Maritime Organization [IMO]. (2006). Resolution MSC.215(82): Performance standard for protective coatings for dedicated seawater ballast tanks in all types of ships and double-side skin spaces of bulk carriers. https://wwwcdn.imo.org/localresources/en/KnowledgeCentre/IndexofIMOResolutions/MSCResolutions/MSC.215(82).pdf
  2. International Organization for Standardization [ISO]. (2006). ISO 8501-3:2006, Preparation of steel substrates before application of paints and related products — Visual assessment of surface cleanliness — Part 3: Preparation grades of welds, edges and other areas with surface imperfections. https://www.iso.org/standard/41021.html
  3. International Organization for Standardization [ISO]. (2007). ISO 8501-1:2007, Preparation of steel substrates before application of paints and related products — Visual assessment of surface cleanliness — Part 1: Rust grades and preparation grades of uncoated steel substrates and of steel substrates after overall removal of previous coatings. https://www.iso.org/standard/43426.html
  4. International Organization for Standardization [ISO]. (2012). ISO 19840:2012, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Measurement of, and acceptance criteria for, the thickness of dry films on rough surfaces.
  5. International Organization for Standardization [ISO]. (2017). ISO 12944-3:2017, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Part 3: Design considerations. https://www.iso.org/standard/64835.html
  6. International Organization for Standardization [ISO]. (2020). ISO 8502-9:2020, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 9: Field method for the conductometric determination of water-soluble salts.
  7. Knudsen, O. Ø., Hagen, C. H. M., Skilbred, A. W. B., Bruaas, T. K., & Nærland, J. (2023). Root causes for corrosion on painted steel structures in marine environments. Materials and Corrosion, 76(6), 802–811. https://doi.org/10.1002/maco.202314046
  8. Marquardt, T., Momber, A. W., Buchbach, S., Kranz, O., Graßl, J., & Viertel, J. (2025). A statistical study into the performance of organic coatings over mechanically prepared welds in a simulated marine environment. Materials and Corrosion, 76(9), 1280–1293. https://doi.org/10.1002/maco.202514864
  9. Momber, A. W., Buchbach, S., Plagemann, P., & Marquardt, T. (2017). Effects of edge treatment parameters on the protection performance of organic coating systems in a wave chamber. Progress in Organic Coatings, 102, 167–177. https://doi.org/10.1016/j.porgcoat.2016.10.010
  10. Morcillo, M. (2003). Soluble salts: Their incidence on the protection of metallic structures by paint coatings. Revista de Metalurgia, 39(Extra), 219–227. https://doi.org/10.3989/revmetalm.2003.v39.iExtra.1123
  11. Shon, M. Y. (2011). Effects of weld fume on the corrosion protection of epoxy coated on carbon steel. Corrosion Science and Technology, 10(3), 80–86. https://koreascience.kr/article/JAKO201121161902206.page
  12. Sørensen, P. A., Kiil, S., Dam-Johansen, K., & Weinell, C. E. (2009). Anticorrosive coatings: A review. Journal of Coatings Technology and Research, 6(2), 135–176. https://doi.org/10.1007/s11998-008-9144-2

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.