Blaming a bad batch and repainting with the same epoxy is the usual response to epoxy paint turning white and powdery, but left in the same sunlight the new film tends to go the same way. What actually lies behind the white powder can be a surface broken down by UV, a missing or weak topcoat, UV-sensitive pigment and binder, amine blush mistaken for chalking, or heat exposure, and sometimes two or more at once.

Background

An epoxy on an outdoor tank or steel frame loses its gloss and fades within a few months, and a hand drawn across it comes away white with powder. When it rains, the powder runs down in white streaks, most visibly on dark colours. This turning of the film surface into a chalk-like powder that rubs off on the hand is called chalking. It is not only a matter of looks: the film gets thinner by whatever falls away as powder, and before overcoating, the powder must be removed for the new film to bond.

UV absorbed by a film breaks bonds and releases radicals, which cut chains or link them excessively, leaving the film soft or brittle. The damage happens at the surface that absorbs the UV, which is why epoxies chalk so readily. A two-part epoxy chalks rather quickly under UV, whereas an aliphatic acrylic polyurethane stays stable (USACE, 1995). The degree of chalking is graded by standard test methods that pick up surface powder on a cloth or tape and compare it with reference photographs (ASTM International, 2015).

So white powder is usually the trace of a binder that has broken down at the surface. Why it broke down differs, though: sunlight, the lack of a topcoat to shield it, a formulation that was weak against UV to begin with, or heat. And it may not be broken-down binder at all, but a different white layer formed during cure.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: note whether the whitened areas face the sun or sit in shade, and whether the change appeared days or months after painting, then check in the paint's technical data sheet, the TDS, whether that epoxy is meant as an exterior finish or as a primer or intermediate coat.

Hypothesis 1: UV breakdown

It can happen on any outdoor equipment where epoxy is left exposed to sunlight, and becomes more pronounced on south- and west-facing sides that get the most sun each day, on upward-facing surfaces, and after the season of strong sun. Walk round a cylindrical tank in a plant yard, for instance: the south side has lost its gloss and leaves powder on the hand, while the north side, shaded by a building, still keeps much of the gloss it had on the day it was painted.

UV damage to epoxy has been confirmed experimentally many times. In a study that exposed unpigmented amine-cured epoxy films without UV stabiliser outdoors and in two UV test devices, there was substantial chemical degradation and thickness loss, chemical change ran ahead of the thickness loss, and nanoscale pits formed at certain surface sites and grew wider and deeper (Rezig et al., 2006). A study of anhydride-cured epoxy by infrared spectroscopy picked up the chemical changes at the irradiated surface and could estimate the thickness of the photo-oxidised layer (Monney et al., 1998). When binder breaks down and falls away from the surface like this, the pigment it held is left behind at the surface and rubs off as powder.

Whether sunlight is the cause shows up well when the sunny and shaded sides of the same equipment are compared. Grade both sides by the tape method, pressing on and peeling off a tape and comparing the powder on it with reference photographs (ISO, 2011), and measure the dry film thickness at the same spots against the application records. If only the sunny side grades poorly and has lost thickness, this hypothesis moves to the front.

UV breakdown itself does not stop for as long as the epoxy is exposed to sunlight, so it is the exposure that needs dealing with. If enough film thickness remains, wash off the powder and apply a UV-resistant topcoat; if a lot of thickness has gone, make up the shortfall with primer or intermediate coat first, then topcoat. If overcoating is not done straight away, grade and measure the sunny sides at intervals and record how fast they are thinning.

Hypothesis 2: weak or no topcoat

There are a few ways epoxy designed as a primer or intermediate coat ends up in the sun for long periods without a proper finish: steelwork left for months in a laydown yard with only primer on because the project was delayed, interior epoxy used on outdoor equipment, and a topcoat applied but of a type that is not UV-resistant. Suppose that on a plant expansion, pipe supports finished in epoxy primer stand outside for nearly half a year before the topcoat stage. On the day the topcoat is due, a hand drawn across them comes away with white powder.

Outdoor coating systems put a topcoat over epoxy to divide the work. The epoxy provides adhesion, chemical resistance and corrosion protection, and the aliphatic acrylic polyurethane above it, with excellent weathering and colour retention, shields it from UV, which is why it is widely used as a topcoat over epoxy primers and intermediate coats in most outdoor environments without chemical exposure. The type of topcoat matters too: aromatic polyurethanes, which contain the benzene ring, darken and yellow in sunlight, and epoxy urethanes, with epoxy in them, tend to chalk. When overcoating an old film that has already chalked, scrubbing the powder off may be all the preparation needed (USACE, 1995).

Laying the specification and the TDS side by side is the first check. Match against the painting records whether the designed system included a topcoat, whether it was actually applied, and if so which resin family the product belonged to. Count from the schedule how long the work stood outside in primer only. If there is a topcoat and powder still forms, look at its family; if it is aromatic or an epoxy urethane, suspect chalking of the topcoat itself.

If the topcoat is missing, the standard course is to remove the powder, check the substrate and apply a UV-resistant topcoat. For overcoating an old film, guidance requires confirming after chalk removal that the surface reaches a rating of at least 8 on the standard scale (DoD, 2021). On projects where primer will sit outside for a long time before topcoating, agree the overcoat window and exposure limit with the supplier from the start, and fit the interval to the topcoat stage within it.

Hypothesis 3: pigment and binder

If films painted at the same place and time chalk at very different rates depending on the product, look at the formulation. This hypothesis comes up when the curing agents differ, with whites and pale colours loaded with titanium dioxide, and after a switch to a cheaper product. An example: two storage tanks standing side by side were painted in the same year with different epoxies, and after the second summer one leaves heavy powder on the hand while the other shows only a faint trace.

Starting with the binder, epoxies also differ in UV resistance depending on the curing agent. Epoxies cured with small polyamines have a strong tendency to degrade under UV and chalk, while polyamide-cured epoxies have much better UV resistance and chalk considerably less outdoors (USACE, 1995). Pigment plays its part too. Titanium dioxide reacts to light at certain sites on the crystal surface and promotes oxidation of the binder, but surface treatment with alumina or silica occupies those sites and inhibits destructive oxidation of the binder; treatments of about 2 to 5% by weight serve general-purpose paints, and about 7 to 10% where more weathering resistance is needed (Allen et al., 2005). Too much pigment relative to binder is also a problem. Beyond the limit at which binder can no longer fill all the spaces between pigment particles, the critical pigment volume concentration, the properties of the film change markedly (Asbeck & Van Loo, 1949).

Judge by the TDS and comparison panels. Check the curing agent family in the TDS, whether the product is meant as an exterior finish, and the solids and pigment information, and ask the supplier for further formulation detail. Paint the two suspect products on the same substrate at the same thickness, set them side by side in the same sunny spot, and grade chalking by the same tape method and measure gloss at set intervals; the difference between products is then recorded in numbers.

Once it narrows to formulation, choose with the supplier a product designed for outdoor exposure from the next job onwards. Even with a different curing agent or pigment, though, epoxy remains a UV-sensitive resin, so for surfaces that get long sun exposure, plan a topcoat in addition to choosing the formulation.

Hypothesis 4: amine blush, not chalk

If a white film appeared within days of painting, and in the shade or indoors at that, look at cure conditions before sunlight. Amine blush is the usual suspect when an ambient-cure epoxy was applied on a cold, damp day, in the evening before dew fell overnight, or in an unventilated space. This fits a floor painted indoors that, entered two days later, looks cloudy and leaves white on the hand when rubbed, yet feels greasy and slick rather than powdery.

Amine blush is a carbonated material formed when the epoxy's amine hardener reacts with carbon dioxide and water vapour in the air (Mills, 2008). During cure, unreacted amine is squeezed out to the film surface and gives a hazy white, but it dissolves in water, so it can be wiped or washed off; it does no harm left in place, but must be removed before another epoxy coat goes on. To reduce it, many manufacturers call for an induction time of 15 to 30 minutes after mixing (USACE, 1995). A study measuring reacting epoxy-amine systems confirmed that carbamate formed by the hardener's reaction with carbon dioxide gathers at the surface and lowers its surface tension (Shenk et al., 2023). It differs from chalking, where binder has broken down in sunlight, in when it appears, what causes it and how it is handled.

Telling them apart is simple. Wipe the white area with a wet cloth: if it dissolves away and the film underneath still has its gloss, it is blush; if dry powder keeps coming off and the surface stays rough and dull after wiping, it is chalking. Check the relative humidity and temperature records for the day of painting and the days after as well. Epoxy coatings cured at 80% relative humidity formed such a surface layer, which a longer induction time after mixing reduced, while at 40% and below the induction time made no measurable difference (Bannister et al., 2022).

If it proves to be blush, wash it off with water and clean cloths and let it dry completely before overcoating. On the next job, observe the TDS induction time, and on days of high humidity or an overnight temperature drop, postpone painting or set the cure conditions with dehumidifying and heating. If blush is the whole story, there is no need to change the paint or add a topcoat because of it.

Hypothesis 5: heat exposure

Briefly consider this hypothesis where ordinary epoxy was applied to hot equipment, such as steam lines, the surroundings of drying ovens and incinerators, or exhaust ducts. It is likely when the design applied the same coating specification as the nearby ambient lines without considering surface temperature in operation, or when a line runs with its insulation removed. Follow the lines out of a boiler room, say, and only those carrying hot steam have faded and roughened, while the ambient lines beside them, painted to the same specification, are sound.

Heat, together with oxygen, oxidises epoxy too. A study that aged two epoxy coatings at five temperatures between 70 °C and 150 °C found carbonyl and amide groups forming in both, with the system cured by a polyether amine more sensitive to oxidation than the one cured by a polyamidoamine (Zahra et al., 2014). Guidance also holds that hot steel such as mufflers and stacks cannot be protected by conventional coatings and calls for specialty coatings selected by the equipment manufacturer (DoD, 2021). On hot outdoor lines that also see the sun, thermal oxidation and UV breakdown attack the surface together.

Measure the surface temperature in operation with a contact thermometer or temperature-indicating labels and compare it with the TDS maximum service temperature. If the damage follows the hot sections rather than the direction of the sun, treat heat as the cause. Once that is confirmed, switch those sections to a heat-resistant coating rated for the maximum surface temperature, chosen on the advice of the supplier and the equipment manufacturer.

Finding the cause

The first thing to separate is blush from chalking. A wet cloth and a strip of tape settle it on site in minutes, and the result changes everything that follows. Next, confirm from the specification and painting records whether there was a topcoat. Formulation comparison and heat measurement need panels or measurements during operation, so they come after.

The next clue is where and when the white areas appeared. If they formed within days, in the shade and indoors as well, look at cure conditions; if they developed over months starting on the sunny sides, look at UV and the topcoat. If products under the same sun change at different rates, suspect formulation, and if the damage tracks only the hot sections regardless of sun, suspect heat.

If that still does not settle it, compare with exposure panels. Of two panels painted with the same epoxy, put a UV-resistant topcoat on one only and expose both to the same sun, along with panels of the other product. Grading by the same tape method, gloss and film thickness at set intervals separates the effect of the topcoat from the difference between products. When a UV test device is used to save time, also check that it ranks the panels in the same order as outdoor exposure.

The final check is to follow the repaired film by the same methods. Record the chalking grade and film thickness of the overcoated surface right after painting and after the first summer, and if the grade holds, take the cause as corrected. Before overcoating, also confirm by the same tape method that the powder was properly removed, since a new film laid over remaining powder does not bond properly.

The hypotheses can overlap. An outdoor epoxy that blushed because it was applied on a damp day and then sits in the sun with no topcoat can show blush first and chalking months later. On hot outdoor lines, heat and UV act together. In such cases wash off the blush first, then settle the exposure, that is, the topcoat or heat-resistant coating to keep out sun and heat, and compare formulations last, because while a white surface layer remains, the other causes are hard to judge accurately.

Limits and cautions

The overcoat window, topcoat type and thickness, and maximum service temperature differ by product, so numeric decisions follow the product's TDS and the coating specification. Whether chalking is only a matter of appearance or the film has thinned enough to lose corrosion protection can be known only by measuring film thickness, and where corrosion has started, agree the extent of repair with the coating inspector. Do not translate results from UV test devices directly into outdoor service life.

When sanding or blasting a chalked film, provide respiratory protection and dust extraction so powder and dust are not inhaled, and if the old film may contain hazardous substances such as lead, check first. Polyurethane topcoats and epoxy hardeners can irritate or sensitise the skin and airways, so follow the product's safety data sheet, the SDS, for gloves, eye protection, respiratory protection and ventilation. Work on hot equipment only after it has been shut down and cooled.

Sources

  1. Allen, N. S., Edge, M., Sandoval, G., Verran, J., Stratton, J., & Maltby, J. (2005). Photocatalytic coatings for environmental applications. Photochemistry and Photobiology, 81(2), 279–290. https://doi.org/10.1562/2004-07-01-RA-221.1
  2. Asbeck, W. K., & Van Loo, M. (1949). Critical pigment volume relationships. Industrial & Engineering Chemistry, 41(7), 1470–1475. https://doi.org/10.1021/ie50475a042
  3. ASTM International. (2015). ASTM D4214-07(2015), Standard test methods for evaluating the degree of chalking of exterior paint films.
  4. Bannister, C., Guy, A., Mihaylova, R., Orgill, J., Burg, S. L., Parnell, A., & Thompson, R. L. (2022). The influence of ambient cure chemistry and stoichiometry on epoxy coating surfaces. RSC Advances, 12(44), 28746–28754. https://doi.org/10.1039/D2RA05067F
  5. International Organization for Standardization [ISO]. (2011). ISO 4628-6:2011, Paints and varnishes — Evaluation of degradation of coatings — Designation of quantity and size of defects, and of intensity of uniform changes in appearance — Part 6: Assessment of degree of chalking by tape method.
  6. Mills, G. D. (2008). Case history: Amine blush in epoxy coatings. Materials Performance, 47(11), 52–55. https://doi.org/10.5006/MP2008_47_11-52
  7. Monney, L., Belali, R., Vebrel, J., Dubois, C., & Chambaudet, A. (1998). Photochemical degradation study of an epoxy material by IR-ATR spectroscopy. Polymer Degradation and Stability, 62(2), 353–359. https://doi.org/10.1016/S0141-3910(98)00018-4
  8. Rezig, A., Nguyen, T., Martin, D., Sung, L., Gu, X., Jasmin, J., & Martin, J. W. (2006). Relationship between chemical degradation and thickness loss of an amine-cured epoxy coating exposed to different UV environments. Journal of Coatings Technology and Research, 3(3), 173–184. https://doi.org/10.1007/BF02774507
  9. Shenk, T. M., Benjamin, K. M., & Winter, R. M. (2023). Impact of carbamate formation on the surface tension of epoxy-amine curing systems. Polymer Engineering & Science, 63(5), 1347–1358. https://doi.org/10.1002/pen.26288
  10. U.S. Army Corps of Engineers [USACE]. (1995). Painting: New construction and maintenance (EM 1110-2-3400). Department of the Army.
  11. U.S. Department of Defense [DoD]. (2021). UFC 3-190-06, Protective coatings and paints. https://www.wbdg.org/FFC/DOD/UFC/ufc_3_190_06_2021.pdf
  12. Zahra, Y., Djouani, F., Fayolle, B., Kuntz, M., & Verdu, J. (2014). Thermo-oxidative aging of epoxy coating systems. Progress in Organic Coatings, 77(2), 380–387. https://doi.org/10.1016/j.porgcoat.2013.10.011

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.