Jonghwan Moon
Product group
Adhesives

When silicone pieces turn up in the oil strainer or filter, it is easy to stop at cleaning the strainer and changing the oil, but if whatever made the pieces is still there, they come back after the next service. What actually produces them can be an oversized bead, a bead in the wrong place, squeeze-out left inside, cured pieces breaking off, or old gasket not fully cleared at reassembly, and sometimes two or more at once.

Background

Not long after its oil pan was refitted with a formed-in-place gasket, a machine shows a low oil pressure warning. With the pan down, strings and thin flakes of silicone are found tangled on the oil pickup strainer, and when the oil filter is cut open, pieces of the same colour are caught between its pleats. The gasket applied at the service has been travelling round the engine.

A blocked intake cuts the oil reaching sliding surfaces that run on an oil film, such as bearings, and a blocked small passage or orifice starves the parts beyond it. Debris in the oil also raises wear on its own. In a test rig simulating a connecting rod bearing, contaminated oil increased wear about twentyfold over clean oil (Ronen et al., 1980). One vehicle maker's service bulletin states that too little oil pan silicone may let oil leak, while too much may contaminate the oil and damage the engine (Ford Motor Company, 2019).

Where the pieces come from depends on how the gasket cures. RTV silicone, which cures with moisture from the air, cures from the surface inwards, so silicone squeezed out inside the joint also turns into rubber strings and skins in time (Comyn et al., 1998). Anaerobic sealant, by contrast, does not cure where air reaches it and cures only between the flange faces, and the excess liquid can mix into the oil and be flushed away (Henkel, n.d.). The pieces that block passages are therefore usually cured silicone or old gasket left from an earlier service.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the pieces from the strainer and filter, record their colour, hardness and shape, and set them beside the technical data sheets, the TDS, and the assembly records of the product used on that joint now and of the one used before.

Hypothesis 1: oversized bead

The more a leak is feared, the thicker the bead tends to get. This hypothesis grows when the tube is squeezed by hand, when the nozzle tip is cut wide, when a joint that once leaked is reassembled, and when an automatic dispenser's output has crept up. Think of a fitter refitting a cover that has leaked before: the nozzle is cut wide, a finger-thick bead of silicone goes round the cover and the bolts are tightened. The silicone that oozed outside is wiped off cleanly with a rag, but the inside of the cover cannot be seen.

When a flange is tightened, the gap between the two faces becomes very thin, and the silicone left over after filling it is pushed out on both the outside and the inside. One manufacturer's design guide gives typical bead diameters for passenger car flanges of 2.5 ± 0.5 mm for RTV and 1.5 ± 0.5 mm for anaerobic, and notes that excess sealant squeezes out on the inner oil side too, where pieces can break off and contaminate the engine oil (Henkel, n.d.). The right size differs by joint. The service bulletin cited above sets a 4.5 mm bead for one particular oil pan and warns that too much can contaminate the oil (Ford Motor Company, 2019). Doubling the bead diameter quadruples its cross-section, so the share the gap cannot take grows that much faster.

Bead size can be measured at the very next assembly. Photograph the bead beside a rule just after applying it or measure its diameter with a bead gauge, and record the amount used per joint by weighing the tube or cartridge before and after. Note where the nozzle tip was cut as well. If a lot oozed outside, assume as much oozed inside, and look along the inner edge with a borescope or a mirror.

If size proves to be the problem, fix the amount. Mark where to cut the nozzle tip for the diameter set by the service instructions or the TDS, and use a metered dispenser on joints that are reassembled often. With automatic dispensing, weigh the output at regular intervals and log it. State in the work standard as well that leaks are prevented by clean faces and assembly within the set time, not by more sealant.

Hypothesis 2: bead in the wrong place

The same amount sends its excess to different places depending on where it is laid. Look at this hypothesis when the bead hugs the inner edge of the flange, when an oil passage crosses the flange face and the bead runs too close round it, and when the bead slid on a face that still carried oil. Hand-applying a timing cover whose oil hole passes through the flange face is such a case. The fitter traces the bead tight round the hole, and when the cover is fitted and tightened, silicone pushed towards the hole sticks to its inner wall as a ring.

The position of the bead decides the path the excess will take. One manufacturer's design guide tells users to lay an RTV bead on the flat flange area about 1 mm from where the inner chamfer begins, and explains that with an inner chamfer the sealant flows along a defined path and fills it, so squeezed-out pieces are not released. The same guide says the bead should pass inside or around dowel and bolt holes without a break, and notes that on oily faces adhesion falls sharply and the bead can slip out of position (Henkel, n.d.). The bulletin cited earlier likewise fixes the bead to straddle the step chamfer and the sealing face (Ford Motor Company, 2019). When the bead sits off towards an oil hole or the inner edge rather than the chamfer, the excess has nowhere to go but straight out to the oil side.

Take out the bead path from the service instructions or drawing and set it against where the bead actually went. On a removed cover, the trace of cured silicone shows the path exactly, so measure how far the bead mark sat from the chamfer and how close it came round each oil hole. Look inside oil holes that cross the flange face for a ring of silicone on the wall, and check what the face was cleaned with before application, and how.

If position is the cause, make the path visible. Keep at the bench a photo or clear template marking the bead path and its distance round oil holes, and lay hand-applied beads against it. Before applying, lift oil from the faces with a lint-free cloth and the specified cleaner, and with automatic dispensing, check the path coordinates and nozzle height at regular intervals.

Hypothesis 3: squeeze-out left inside

Silicone that oozes outside is noticed and wiped, but what oozes inside is usually left where it is. Squeeze-out inside grows larger and comes away more easily when a part is set down at an angle and slid into place, when a cover is fitted, lifted off and fitted again, when assembly happens after the surface has begun to skin, and when oil is filled and the engine run straight after assembly. Consider a pan set down wrongly once in a dry winter workshop, lifted and set again. Smeared silicone spreads along the inner edge as a thin film, and some of it stretches into strings that sag into the pan.

Silicone left inside is a hazard because of the way it cures. In moisture-cure silicone, water passing through the outer layer already cured goes on to cure the next layer, so the cured depth grows with the square root of time (Comyn et al., 1998). In a study of a one-part silicone, cure took longer the lower the humidity (Elsmore & De Focatiis, 2021). Strings and films sagging inside a closed housing can stay soft inside with only a cured skin, and once oil starts to circulate, the flow drags them loose. A manufacturer's guide calling for assembly before the surface skins over, and a service bulletin requiring the oil pan to be fitted within 10 minutes of applying the bead, can be read in the same light (Ford Motor Company, 2019; Henkel, n.d.).

Checking starts by retracing the work sequence. Ask the fitters how long passed between applying and assembling, whether a part was refitted, and how long it was from assembly to filling oil and starting, and set these against the skin-over time and cure time in the TDS. If the joint can be opened, look along the inner edge for smeared film, hanging strings and folded bead, and see whether the pieces from the strainer match the shape of those strings or films.

If squeeze-out left inside is the cause, change the assembly movement. Lower the part straight onto dowels or guide pins and seat it in one go, and if it was placed wrongly, do not tighten it as it is but strip the bead and apply a new one. Wipe off any inside squeeze-out within reach before it cures, assemble within the time set by the TDS, and respect the TDS cure time before filling with oil and running. In dry seasons allow that much longer.

Hypothesis 4: detached cured pieces

If pieces appear although the joint has not been opened recently, they may be silicone that cured long ago and has broken away. The likely places are equipment with long running hours, flanges always immersed in hot oil, designs that fill a groove with sealant, places such as T-joints where sealant goes in as a lump, and thin covers whose flanges move slightly in service. At an oil change on a machine several years old, faded pieces of silicone come out at the drain plug and the strainer. The service records show that the joint has never been opened since factory assembly.

Cured silicone also changes in oil. In a study of the effect of engine oil additives on silicone rubber, specimens soaked in oil at 150 degrees Celsius lost much of their tensile strength in the presence of ZDDP, an anti-wear additive, with acidic phosphorus compounds appearing to be the main cause (Kusuhara et al., 2017). In another test that soaked RTV silicone in hot engine oil, hardness fell by about 30% and volume swelled by about 20% (Herman & Donaldson, 2020). Design plays a part too. One manufacturer's design guide advises against grooves for RTV because trapped sealant cures slowly and excess squeezes out to the oil side, where it can break off, and explains that an inner chamfer stops squeezed-out pieces from coming loose (Henkel, n.d.). A thin silicone lip hanging on the oil side, swollen and weakened by oil and worked by the flow and by flange movement, can eventually tear away.

The look of a piece hints at its age. Faded, swollen pieces with rounded edges have most likely been in oil a long time, while pieces with bright colour and sharp torn edges are most likely recent. Match the colour and hardness of the pieces with the product used at factory assembly and the one used in service, and check on the drawing whether the joint is designed with a groove or a chamfer. If the oil and sealant are suspected of not getting on, commission the standard tests that soak rubber specimens in oil and measure changes in volume, hardness and tensile properties, using the oil actually in service (ASTM International, 2020; ISO, 2024).

If cured pieces breaking off looks likely, open the joint at the next service, remove every silicone lip hanging inside, and choose an oil-resistant grade suited to the running temperature and oil with the sealant supplier. Add a strainer and drain plug check to the checklist for every oil change to watch whether pieces return. Where the design can be changed, consider an inner chamfer in place of a groove.

Hypothesis 5: old gasket left behind

On a reassembly job, the old gasket may deserve suspicion before the new one. Old gasket finds its way into the engine when scrapings fall into the housing as old silicone is lifted, when faces are ground with abrasive discs or wire brushes, and when work goes ahead without plugging oil passages and housing openings. Picture old silicone being scraped off the block face. A few scrapings drop inside the crankcase, out of reach, so they are left, fresh silicone is applied and the pan goes on.

Whatever comes off the face ends up wherever oil goes. One vehicle maker's service bulletin shows debris from abrasive cleaning collected on a crankshaft deflector and states that once it gets there it can be spread to any surface in the engine, and it warns that the fine grit from abrasive pads cannot be removed by the oil filter. The same bulletin recommends spraying on a cleaner, letting it soak for several minutes and lifting the material with a plastic scraper (General Motors, 2024). A cleaner works because silicone takes up solvent and swells, and in a study that soaked silicone rubber in many solvents, the degree of swelling varied with the solvent's solubility parameter (Lee et al., 2003). Soaked and lifted, old silicone comes off in large films that are easy to collect, but scraped or ground dry, it breaks into small crumbs and dust that scatter.

Colour is the clue. Pieces whose colour differs from the newly applied product, or pieces mixed with metal particles or abrasive grains, most likely come from the old gasket and the cleaning work. Ask the fitters which tools were used to clean the faces and whether openings were plugged during the work. Using the method in the vehicle component cleanliness standard, which washes particles off a part, filters them and measures their size and number, lets the particles left in a cleaned housing be compared in figures (ISO, 2018).

When the pieces trace back to old gasket, change the cleaning sequence. Plug oil passages and housing openings with tape or caps before scraping, soak old silicone with a cleaner and lift it in large films with a plastic scraper. Use no abrasive discs or wire brushes on the faces of parts that see oil. Afterwards, wipe inside the housing with a lint-free cloth to confirm no crumbs remain, and on reassembled equipment check the oil filter and strainer once more after the first run.

Finding the cause

The most telling evidence is already in hand: the pieces collected from the strainer and filter. Simply matching their colour with the product in use now and the one used before usually separates pieces from the new gasket and pieces from the old. Records come next. Find in the service records and from the fitters when the joint was opened, which product went on and how much, and how long after applying it the joint was assembled and filled with oil.

The shape of the pieces points further. Thin strings and films in bright colour come from squeeze-out left inside or an oversized bead, and rings that match a hole diameter come from a bead laid close to an oil hole. Faded, swollen pieces with rounded edges from a joint not opened recently point to cured pieces breaking off, and crumbs of another colour mixed with metal particles or abrasive point first to old gasket left from cleaning.

If that still does not settle it, make the next assembly the control trial. Assemble by a set sequence in which the bead diameter and amount are measured, the bead path is photographed, the application and assembly times are logged and openings are plugged before cleaning, then inspect the strainer and filter after the same running time. Changing one thing at a time shows which change reduced the pieces.

The final check is the oil system after running. After the set running time, open the strainer and filter to confirm no pieces are present, cutting the filter open to inspect between the pleats if needed. The cause has been put right only when oil pressure is back in its normal range and no pieces appear at the next oil change either. If there was bearing noise or a pressure warning, do not stop at removing the pieces; check the condition of the bearings as well.

The hypotheses can overlap. When a fear of leaks makes the bead thick, the bead is laid against the inner edge, and the part is set down wrongly once and seated again, squeeze-out inside grows for three reasons at once. In such cases, tie amount, path and assembly time into one work standard and correct them together, and first clear out the pieces and old crumbs already inside the engine, or the effect of the correction cannot be judged properly.

Limits and cautions

Bead diameter, bead path, skin-over time and the cure time before oil filling differ by product and joint, so numeric decisions follow the product's TDS and the equipment maker's service instructions. If an oil pressure warning appears or a bearing becomes noisy, stop running at once, and leave the assessment and repair of bearing and crankshaft damage to an engine specialist. Do not let a trial run after clearing the pieces stand in for that judgement.

Safety matters too. For gasket removers and cleaners, follow the product's safety data sheet, the SDS, for protective equipment and ventilation. Oil and housings are hot just after running, so let them cool before opening, and when lowering an oil pan or cover, stop the equipment completely, lock it out and support the part. Dispose of used oil, oily rags and removed filters under the local waste rules.

Sources

  1. ASTM International. (2020). ASTM D7216-20, Standard test method for determining automotive engine oil compatibility with typical seal elastomers. https://store.astm.org/d7216-20.html
  2. Comyn, J., Day, J., & Shaw, S. J. (1998). Kinetics of moisture cure of silicone sealants. The Journal of Adhesion, 66(1–4), 289–301. https://doi.org/10.1080/00218469808009970
  3. Elsmore, M. T., & De Focatiis, D. S. A. (2021). Combined roles of temperature and humidity on cure of a silicone elastomer. Polymer Testing, 93, 106967. https://doi.org/10.1016/j.polymertesting.2020.106967
  4. Ford Motor Company. (2019). 2.7L EcoBoost: Oil pan leaking (Technical Service Bulletin 19-2205). Copy published by the U.S. National Highway Traffic Safety Administration. https://static.nhtsa.gov/odi/tsbs/2019/MC-10164470-0001.pdf
  5. General Motors. (2024). Use of surface conditioning disks when cleaning gasket sealing surfaces and/or reused parts (Service Bulletin 00-06-01-012N). Copy published by the U.S. National Highway Traffic Safety Administration. https://static.nhtsa.gov/odi/tsbs/2024/MC-11006670-0001.pdf
  6. Henkel. (n.d.). Leak-free flanges: A Loctite design guide. https://dm.henkel-dam.com/is/content/henkel/Gasketing%20Design%20Guide-Final_LR
  7. Herman, J., & Donaldson, K. (2020). Experimental investigation on the impact of engine oil on RTV silicone (SAE Technical Paper 2020-01-5002). SAE International. https://doi.org/10.4271/2020-01-5002
  8. International Organization for Standardization [ISO]. (2018). ISO 16232:2018, Road vehicles — Cleanliness of components and systems. https://www.iso.org/standard/70267.html
  9. International Organization for Standardization [ISO]. (2024). ISO 1817:2024, Rubber, vulcanized or thermoplastic: Determination of the effect of liquids. https://www.iso.org/standard/86602.html
  10. Kusuhara, S., Yoshimura, K., Kunieda, K., Suzuki, N., Matsuki, S., & Shitara, Y. (2017). Experimental investigation on the influence of engine oil additives on silicone rubber. SAE International Journal of Fuels and Lubricants, 10(2), 461–468. https://doi.org/10.4271/2017-01-0877
  11. Lee, J. N., Park, C., & Whitesides, G. M. (2003). Solvent compatibility of poly(dimethylsiloxane)-based microfluidic devices. Analytical Chemistry, 75, 6544–6554. https://doi.org/10.1021/ac0346712
  12. Ronen, A., Malkin, S., & Loewy, K. (1980). Wear of dynamically loaded hydrodynamic bearings by contaminant particles. Journal of Lubrication Technology, 102(4), 452–458. https://doi.org/10.1115/1.3251580

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.