Applying another coat over the cracks is the usual response when firestop sealant cracks as it dries, but if the conditions that cracked it remain, the new layer tends to go the same way, and fire performance can only be expected when the tested configuration is followed. What actually lies behind it can be drying shrinkage of a water-based product, a gap that is too wide, a product too stiff for joint movement, drying in the cold, or poorly prepared faces with dust and oil left on them, and sometimes two or more at once.

Background

A few days after red firestop sealant was packed into the openings where pipes and cables pass through walls and floors, and into the joints between wall heads and slabs, the work is checked again. Fine crazing has spread over the surface like a web, the edges have pulled away from the wall to leave visible gaps, and in some openings the sealant has dropped out in lumps onto the floor. A surface that was smooth when filled has changed this way as it dried.

Firestop sealant is the barrier that keeps flame, smoke and hot gases from passing into the next compartment in a fire. A crack or gap is a ready path for smoke, and a spot where sealant has fallen out is as good as an open hole. When an inspection flags it, the work must be removed and redone, so finishing trades and handover slip with it; if it goes unnoticed, the compartment cannot do its job in a fire.

The performance of a firestop sealant comes not from the sealant alone but from the whole tested configuration. The type of wall or floor, the item passing through, the size of the gap, the backing and the depth of sealant are tested as one set, and site inspection confirms that what was installed matches the documents for that set (ASTM International, 2024b). Intumescent firestop sealants contain material that swells into an insulating layer when exposed to fire, so they must stay attached to the faces without gaps after drying in order to swell in place when fire comes (Weil, 2011).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph the cracked or detached spots, measure the gap width and the sealant depth, note the temperature and humidity on the day of installation and for the few days after, and compare all this with the sealant's technical data sheet, the TDS, and the drawing of the listed system.

Hypothesis 1: drying shrinkage

Look at this hypothesis where a water-based acrylic firestop sealant, which hardens by giving off water, has been packed deep or thick in one go. The water that leaves during drying is lost volume, so the more sealant was placed, the larger the effect. Picture walking round the next morning after filling a number of wall penetrations in a single day. The middle of the sealant has sunk into a saucer-like dip, a crack runs along its floor, and at a few points the edge has come slightly away from the wall of the opening.

Water-based sealants harden mainly as their water evaporates, and they lose volume to match. The standard test for volume shrinkage calculates it from the density of freshly extruded sealant and the weight lost in drying, and uses the value to predict the shape the cured sealant will take in the joint (ASTM International, 2022). Inside, the sequence runs as follows. As water leaves, the polymer particles pack against one another, and the capillary forces of the water left between them pull the whole layer to contract. The layer is stuck to the faces and cannot shrink sideways, though, so that pull builds up as tensile stress, and when the stress exceeds what the layer can bear, it cracks (Routh, 2013). Latex films have a limiting thickness at which cracking begins, so the thicker the layer beyond it, the more prone it is to crack as it dries (Tirumkudulu & Russel, 2005).

The shape of the cracked sealant is the first clue. Check whether the middle has sunk into a dip, whether the cracks are spread evenly over the surface, and how deep they go, probing with a knife point. Next, find in the TDS whether the product is water-based and what it says on solids content and shrinkage, then measure the actual fill depth and compare it with the depth the system specifies and the thickness that may be placed in one go. If other spots filled shallower with the same product are sound, the weight of evidence shifts to this hypothesis.

If drying shrinkage is the cause, fill with the coming loss in mind. Keep to the depth the system requires, but place it in stages so no layer exceeds the single-pass thickness set in the TDS, and confirm with the system drawing and the supplier whether topping up is permitted. A higher-solids product that shrinks less is another route, but check first that the replacement is in the same listed system. Where cracks have formed after drying, remove the cracked part and refill rather than coating over it.

Hypothesis 2: gap too wide

Suspect this hypothesis when a core hole was drilled much larger than the pipe, when the pipe sits off to one side so the opposite side gapes, when building tolerances have left a joint wider than designed, or when a gap was filled with sealant alone and no backing. It shows up where a pipe runs against one wall of a core hole far larger than its diameter. The narrow side is sound, but on the wide side, open enough to take a few fingers, the sealant has sagged and cracked deeply.

A listed system sets the minimum and maximum annular space, the gap around the pipe, together with the backing and the sealant depth, and was tested only within those limits, so a gap outside them is a configuration that has never been tested. Site inspection, too, checks the installed gap and depth against the system documents (ASTM International, 2024b). Physically, a wide gap is also at a disadvantage. Filling it with sealant alone puts more material in one place, and the more water that has to leave, the more the sealant shrinks (ASTM International, 2022). Thicker layers crack more readily as they dry (Tirumkudulu & Russel, 2005), so with the same product the wide side tends to crack first, and uncured sealant with nothing beneath it cannot carry its own weight and sags.

Take a rule and a depth gauge and measure the gap at several points around it. Record both the narrowest and the widest points, and lift a little sealant at one side to see whether the backing sits at the specified depth. Set these values against the gap range on the system drawing and see whether the cracked spots coincide with the parts beyond that range.

When the gap exceeds the system range, more sealant will not fix it. Find another listed system for that gap size, or repair the opening to bring it within range, fit the backing as drawn and fill only to the specified depth. Where no system fits, obtain an engineering judgement from the supplier and agree it with the inspecting authority in advance. On future work, sizing core holes to the pipe is the simplest prevention.

Hypothesis 3: too stiff for movement

Where the joint width grows and shrinks, as at joints between wall heads and slabs, curtain wall edges and building movement joints, weigh movement first. The same applies to penetrations carrying pipes that expand and contract with hot water, or that vibrate. Pay closer attention if a low-elasticity penetration product, or one that sets hard like mortar, was used in such places. A typical picture: on an upper floor of a steel-framed building, penetration-grade firestop sealant was packed into the joint between a lightweight wall head and the deck, and a few weeks after loads from the floors above began to bear on it, a single crack opened along the joint and the sealant came away from one face.

The width of a joint changes with load, temperature, wind and building sway, and the sealant inside it has to stretch and compress each time. Elastomeric joint sealants are classified by how far, as a percentage of joint width, they can extend and compress without failing (ASTM International, 2018). Fire-resistive joint systems can be tested for repeated movement alongside the fire test, and the results hold only up to the movement conditions tested (ASTM International, 2024a). When movement exceeds what the product can follow, the sealant tears through its body as the joint opens, or the weakest bonded face lets go first. In a water-based product already under drying shrinkage stress, the added movement can make it crack sooner.

First decide whether the spot is a moving joint or a static penetration. If it is a joint, look in the TDS and system documents for whether the product and system were movement-tested for joints and what movement value they carry. Mark both sides of the joint and measure how its width changes with season and load to put the actual movement into numbers. A single crack running the length of the joint that widens over time points strongly to movement.

If the joint really is moving, changing the product is not enough; the system must change. Choose a joint system tested to a movement value larger than the expected movement, and size the joint so the movement stays within the share the sealant can take. The standard guide on joint sealants likewise treats joint design together with surface preparation (ASTM International, 2016). Where a penetration product has gone into a joint, remove it and reinstall with a joint system.

Hypothesis 4: cold drying

Winter work, buildings not yet heated, floors before the windows go in, and basements and shafts without ventilation are where cold deserves suspicion. High humidity on top of low temperature makes it more likely. Say penetrations were filled late on a midwinter afternoon on a floor still open to the outside. Overnight the temperature falls close to freezing, and a few days later the surface looks hard but crumbles under the hand and is covered in fine cracks.

For a water-based sealant to become a continuous rubber layer, the polymer particles must deform against one another once the water has gone, and chains must cross between touching particles to join them into one. The lowest temperature at which this happens is called the minimum film-forming temperature, and below it the particles cannot join, so the film cracks and crumbles like powder (Keddie, 1997). Low temperature and high humidity also slow the evaporation of water itself, so the inside stays wet long after the surface looks dry (Steward et al., 2000). If it freezes or takes load in the meantime, the still-weak layer cannot hold.

Find the temperature and humidity on the day of installation and for several days after in the site diary or nearby weather records, and compare them with the minimum application temperature and curing conditions in the TDS. Cut out a piece of sealant to see whether the inside is still wet and soft, and whether it crumbles to powder when rubbed between the fingers. If the same product went in on a heated floor on the same day, compare the two side by side. Check the temperature where the material was stored as well.

If cold appears to be the cause, remove the crumbling or cracked sealant and refill. Work within the TDS application temperature range when refilling, use temporary heating and enclosure so that temperature holds until curing is complete, and ventilate so the moisture can escape. Store the material somewhere warm until use, and in winter schedule the work for the warm part of the day rather than late afternoon.

Hypothesis 5: poor surface prep

Suspect the faces when sealant comes away from them whole rather than cracking. Typical culprits are slurry dust left on the wall of a core hole straight after drilling, the weak cement skin on a concrete surface, formwork release agent, oil and cutting fluid on pipe surfaces, and damp faces. Take an opening where the pipe went in and the sealant was packed as soon as the core was drilled: grey dust still sits on the wall of the hole. As the sealant shrank on drying, it came cleanly away from that wall to leave a gap all round, and the back of the removed sealant carries the dust.

Sealant must be firmly bonded to the faces to withstand the pull of drying shrinkage and the movement of the joint. With dust or oil on the face, the sealant bonds to that layer instead, and the layer only rests loosely on the face, so under load it parts at this weak boundary layer. A classic analysis explains poor adhesion by such weak boundary layers (Bikerman, 1967). A water-based sealant pulls on its bonded faces as it shrinks during drying, so if the faces are not clean, it can come away before any other force is added. This is why the guide on using joint sealants treats surface cleaning and priming as part of the installation procedure (ASTM International, 2016).

Start with the back of the detached sealant. If dust, oil or traces of release agent are on it, and the face shows no sealant residue, the faces are the likely cause. Where sealant is still attached, confirm with a field adhesion test, cutting part of the sealant and pulling it by hand. The test looks at whether the sealant tears through its body or parts from the bonded face, and an easy release from the face points to surface preparation (ASTM International, 2019). On pipe surfaces, wetting with water and watching whether it spreads evenly or beads up gives a sense of an oily film.

Once surface preparation proves to be the problem, put the faces right before refilling. Brush down the walls of the opening, vacuum out the dust and scrape off any weak cement skin. Wipe oil from pipes by the method the TDS recommends and let everything dry fully before filling. Where the product and face call for primer, never skip it, and change the sequence from filling straight after core drilling to filling only after cleaning and drying are complete.

Finding the cause

There is no need to test all five hypotheses from the outset. Rule out first what can be checked straight away with eyes, a rule and the records. Whether the product is water-based and its minimum application temperature are in the TDS, the weather on the day is in the site diary, gap width and depth can be measured with a rule, and the back of detached sealant only needs to be looked at. Joint movement has to be measured over time, so it comes next.

The pattern of cracking narrows the cause a long way. A middle sunk into a dip with fine cracks across the whole surface points first to drying shrinkage. Sagging and cracking only on the wide side of one opening suggest gap size, and a single crack along a joint that widens with time suggests movement. Crumbling to powder under pressure points to drying in the cold, while sealant that parts cleanly from the face rather than cracking, with dust or oil on its back, points to contaminated faces.

If that still does not settle it, make small control installations. With the same product on the same day, fill one to the specified depth and one deeper, and one after cleaning and drying the faces and one as found. Placing one in a warm spot and one in a cold spot is another option. Vary only one condition at a time, or there is no telling what made the difference, and compare cracking and detachment a few days later on the same basis.

After the repair, go back a few days and a few weeks later to see that no cracks or gaps have returned. Make the final check the way site inspection does, comparing what was installed with the documents for the listed system (ASTM International, 2024b). The job is done only when gap size, backing, depth and product all match the drawing and the sealant stays attached to the faces without gaps after drying.

The hypotheses overlap easily. Filling a wide gap on a cold day leaves a lot of water to remove at a slow drying rate, so shrinkage and cold reinforce each other, and a dusty face lets go as soon as drying shrinkage pulls on it. In such cases, fix first what can be put right before installation, such as gap size and the state of the faces, then match application temperature and fill thickness. In a moving joint, check that the system, not just the product, is right before anything else. Only then can the remaining cause be identified properly.

Limits and cautions

Gap range, backing, sealant depth, movement value and application temperature differ by listed system and product, so numeric decisions follow the system drawing and the TDS. When changing to a configuration not in the system, or dealing with a spot no system fits, do not decide on site judgement alone; get the supplier's engineering judgement and confirmation from the building and fire authorities having jurisdiction and the inspector.

Safety matters too. For sealants, primers and cleaners, follow each product's safety data sheet, the SDS, for protective equipment and ventilation. Dust from core drilling or grinding concrete can contain crystalline silica, which harms the lungs when breathed in (OSHA, n.d.). Use wet methods or dust extraction with suitable respiratory protection, and work on high penetrations and joints only with fall protection in place.

Sources

  1. ASTM International. (2016). ASTM C1193-16, Standard guide for use of joint sealants. https://store.astm.org/c1193-16.html
  2. ASTM International. (2018). ASTM C920-18, Standard specification for elastomeric joint sealants. https://store.astm.org/c0920-18.html
  3. ASTM International. (2019). ASTM C1521-19, Standard practice for evaluating adhesion of installed weatherproofing sealant joints. https://store.astm.org/c1521-19.html
  4. ASTM International. (2022). ASTM C1241-14(2022), Standard test method for volume shrinkage of latex sealants during cure. https://store.astm.org/c1241-14r22.html
  5. ASTM International. (2024a). ASTM E1966-24, Standard test method for fire-resistive joint systems. https://store.astm.org/e1966-24.html
  6. ASTM International. (2024b). ASTM E2174-24, Standard practice for on-site inspection of installed firestop systems. https://store.astm.org/e2174-24.html
  7. Bikerman, J. J. (1967). Causes of poor adhesion: Weak boundary layers. Industrial & Engineering Chemistry, 59(9), 40–44. https://doi.org/10.1021/ie51403a010
  8. Keddie, J. L. (1997). Film formation of latex. Materials Science and Engineering: R: Reports, 21(3), 101–170. https://doi.org/10.1016/S0927-796X(97)00011-9
  9. Occupational Safety and Health Administration [OSHA]. (n.d.). Silica, crystalline. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/silica-crystalline
  10. Routh, A. F. (2013). Drying of thin colloidal films. Reports on Progress in Physics, 76(4), 046603. https://doi.org/10.1088/0034-4885/76/4/046603
  11. Steward, P. A., Hearn, J., & Wilkinson, M. C. (2000). An overview of polymer latex film formation and properties. Advances in Colloid and Interface Science, 86(3), 195–267. https://doi.org/10.1016/S0001-8686(99)00037-8
  12. Tirumkudulu, M. S., & Russel, W. B. (2005). Cracking in drying latex films. Langmuir, 21(11), 4938–4948. https://doi.org/10.1021/la048298k
  13. Weil, E. D. (2011). Fire-protective and flame-retardant coatings – A state-of-the-art review. Journal of Fire Sciences, 29(3), 259–296. https://doi.org/10.1177/0734904110395469

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.