KALTECKOREA

BlogApplication notes

Why do rubber and plastic parts smell and fog glass?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Release & Process Aids

Airing parts for a while is the usual response when they smell or fog glass, but concentrations lowered that way climb again as temperature rises, so unless what keeps coming out of the part is found, the problem returns. What actually lies behind it can be volatile light oil, under-cured rubber, hot storage, too much oil or other additives, and sometimes two or more at once.

Background

A quality engineer at a carmaker calls. Customers have complained that cars parked in the sun all summer have an oily, cloudy film on the inside of the windscreen, and that the cabin smells of rubber when the door opens. Then comes word that the door seals, mats or trim skins supplied had been tested and their fogging values exceeded the limit.

Fogging blocks the driver's view, which makes it a safety issue, and odour spoils the first impression of a new car and comes back as returns and claims. Failing a customer's interior air requirements delays part approval, and lots already shipped may have to be retested or replaced. The same problem can appear well beyond cars, wherever a warm space meets cool glass: rubber parts inside appliances, the inside of lamp covers, sealed display cabinets.

Fogging is defined as the condensation on glass of volatile components evaporated from vehicle interior materials, and the standard tests heat a sample and measure the condensate on a cool glass plate either by loss of gloss or by weight (DIN, 2011). Odour has the same root. Small molecules in a polymer, such as oils, plasticisers, curative decomposition products and catalysts, migrate to the surface and pass into the air, and the semi-volatile ones with higher boiling points tend to condense on cool surfaces rather than stay airborne. For these semi-volatiles, the gas concentration just above the material surface sets the emission rate, so they keep coming out slowly for a long time (Xu & Little, 2006).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: gather the formulation, raw material lots, cure conditions and storage history for a problem lot and a good lot, and set the customer's test method and conditions beside values in the raw materials' technical data sheets, the TDS, such as volatile content and flash point.

Hypothesis 1: volatile light oil

This hypothesis comes up after the process oil in rubber or the plasticiser in plastic has been switched to a lighter grade for cost or processing. It also arises when the raw material supplier changes, when a product with the same name has a different distillation range, or when a little light oil was blended in to lower viscosity. Suppose process oil was moved to a new source to save cost, and a few months later the first fogging complaint arrived. The recipe is unchanged and hardness and tensile strength are within specification, so nobody thinks of that change.

The smaller the molecule, the higher its vapour pressure and the more easily it evaporates at a given temperature. Oil molecules evaporating from a warm part spread into the cabin air, then meet cooler glass and condense into tiny droplets that scatter light. That is why a key property carmakers ask for when choosing plasticisers for interior trim is low volatility and the low fogging that goes with it, and why plasticisers of different molecular structure differ even within one family (Wadey & Holzmann, 1987). Industry test methods split this property by boiling range. A sample is heated at 90 °C to obtain the volatile organic compound value from what comes out, then at 120 °C to obtain the fogging value, which counts substances boiling in the range of alkanes with roughly 14 to 32 carbon atoms (VDA, 2011). The lower-boiling fractions of a light oil can fall within this range.

Compare the raw materials first. Set the distillation range, viscosity, flash point and heating loss from the certificates of the oil or plasticiser used in the problem lot and the good lot side by side, and if raw material remains, measure heating loss again under the same conditions. For the part, identify what comes out by thermal desorption gas chromatography with mass spectrometry: a row of alkanes in the fogging range points to oil, a large peak of a particular ester to plasticiser. Compare the fogging value itself by the customer's test method, through gloss loss or weight of condensate on the glass plate.

If light components are the cause, add an upper limit on distillation range or heating loss to the raw material specification, and make a fogging test a condition of approval whenever the source changes. For a material already switched, consider going back to a heavier oil grade or a higher molecular weight plasticiser, and confirm by compound trials, since low-temperature flexibility and processing change with it.

Hypothesis 2: under-cured rubber

Suspect this hypothesis when cure time has been cut to raise output, when temperature varies from place to place in a mould or extrusion curing line, when the core of a thick part heats more slowly than its skin, and when a compound change was not followed by new cure settings. All the more so if odour complaints cluster in parts from one cavity of a mould or one section of an extrusion line. Those parts may also feel slightly soft under the thumb, with a faintly tacky surface.

Vulcanisation builds bridges between rubber chains to form a network. In sulphur cure, accelerators and activators first react with sulphur to form intermediates, which attach to the rubber chains and then turn into crosslinks between them over several steps, and how far the reaction goes is set by temperature and time (Coran, 1994). With too little time or too low a temperature, the part leaves the mould with these steps unfinished, so more curatives and accelerators that never became crosslinks, along with their intermediates and decomposition products, can remain in the rubber. A loosely knit network also holds small molecules such as oil less firmly. Whatever remains creeps to the surface each time the part warms and becomes odour and condensate.

Read the state of cure with a curemeter. Load uncured compound of the same recipe into a rotorless curemeter and record the torque curve over time; the time for torque to finish rising and the maximum torque can then be set against the actual process conditions (ISO, 2018). Measure the real temperature at each mould position with a thermocouple or surface thermometer, and for thick parts cut a section and compare hardness at core and skin. Heating a problem part and a good part under the same conditions and comparing odour and fogging values is another quick check.

When under-cure is confirmed, reset cure time and temperature to match the curemeter curve, and fix cold mould positions and curing line sections. Set time for thick parts so the core cures fully. For parts with strict customer limits, review with the raw material supplier a post-cure, further heating in an oven after vulcanisation, to drive off remaining volatiles, and check the change in physical properties along with it.

Hypothesis 3: hot storage

The core of this hypothesis is where a part has been and for how long since it was made. Complaints of odour and fogging rise for parts that passed through places that heat up or trap air: warehouses under the roof in summer, container shipping, sunny dispatch bays, sealed packaging. Look this way if parts made from the same compound by the same process were fine when delivered in winter but only those sent by container in midsummer failed. Odour rushes out as soon as the box is opened, and a cloudy film may sit on the inside of the plastic wrap.

As temperature rises, the vapour pressure and mobility of small molecules in the material rise together and emission speeds up. In a study that followed a new car's cabin air for over three years, the concentrations of most compounds fell over time but rose again with interior temperature, and interior temperature and days since delivery were the main factors setting them (Yoshida & Matsunaga, 2006). In tests on plasticisers in vinyl flooring and crib mattress covers, emissions also rose markedly with temperature (Liang & Xu, 2014). Inside a sealed box or wrap, what comes out has nowhere to go, so the concentration builds and spreads all at once when the box is opened. Condensate forming on cool inner surfaces of the packaging as warm parts cool down follows the same principle as fogging on glass.

Checking starts by retracing the storage history. Find when the problem lot was made, which warehouses and transport it passed through, and whether there are season and temperature records for that period, and if possible put a temperature logger in a box to follow the next shipment. Testing parts from the same lot kept somewhere cool alongside parts that went through heat shows the difference. Compare odour under the customer's sensory test conditions; the industry method places a sample at a set condition of 23 °C, 40 °C or 80 °C, and trained assessors grade it on a scale from 1 to 6 (VDA, 2022).

When storage turns out to be behind it, the first job is to cut the time parts spend hot. Keep them somewhere cool and ventilated, rethink routes and packaging for summer shipments, and limit sealed packaging to where it is really needed. Keeping parts cool does not make the substances inside disappear, though, so if there is little margin against the customer's limit, deal with the other hypotheses as well, especially the oil side.

Hypothesis 4: too much oil

This is about the amount of oil rising while its type stays the same. Look at this hypothesis in compounds where filler and oil were raised together to lower hardness, ease processing or use less expensive rubber. Batches in which a weighing error let in more oil than specified belong here too. Picture a plant that has moved to a new cost-saving compound with less rubber and correspondingly more oil. Before long the part surface feels slippery on the fingers, and the condensate weight climbs in testing.

More oil means more molecules available to reach the surface, and the gas concentration just above it stays high, so emission lasts longer (Xu & Little, 2006). Rubber and filler can hold only so much oil, and oil beyond that bleeds to the surface, forming a film that feeds odour and condensate. With that much condensate, gloss alone may not read the amount properly. Condensate with low surface tension or a heavy film can mislead the gloss measurement, and in those cases the gravimetric method is preferred (ISO, 2021).

Check the formulation against the weighing records to confirm how many parts of oil actually went in, and for suspect batches measure the extractable content of the part by solvent extraction and compare it with a good batch. Warming the part on clean paper or a glass plate and looking for an oil mark gives a simple read on bleeding. For fogging tests, recording both the gloss value and the condensate weight makes the effect of oil level easier to read.

If oil is judged excessive, lower the oil level in the compound and recover the resulting change in hardness and processing through filler type or another way of plasticising. If a weighing error is to blame, calibrate the oil dosing equipment and record the amount added in every batch. When setting oil level, include the customer's fogging and odour limits as test items from the start, not just physical properties.

Hypothesis 5: other additives

If the oil has not changed and cure is normal yet the part smells, turn to the remaining additives. Peroxide crosslinkers, polyurethane foaming catalysts, antioxidants, and the release agents and processing aids that help parts leave the mould are all candidates. This hypothesis moves forward when people say the character of the odour changed after a crosslinker was switched to another supplier's or a release agent was changed in moulding. Some describe it as sweetish or fishy, unlike the usual rubber smell.

The crosslinking reaction itself can leave odorous substances behind. Dicumyl peroxide, a peroxide widely used to crosslink rubber, forms acetophenone as it decomposes, and because this sometimes causes rubber odour problems, other peroxides with fewer odorous decomposition products are used instead (Nakamura, 2006). This happens even with full cure, so it needs to be told apart from under-cure. A study that searched for odorants in fifteen polyurethane samples identified 50, including tertiary amines, fatty acid oxidation products, short-chain aldehydes and phenol derivatives, and one of them, 1,4-dimethylpiperazine, had been used as a catalyst. The same study judged that acetaldehyde and propanal were continuously regenerated in the material (Minig et al., 2024). A single additive or its decomposition product can dominate the odour, in other words, and can return even after airing.

Narrow down the source of the odour with instruments. Run the problem part and a good part through thermal desorption gas chromatography with mass spectrometry under the same conditions, and look for peaks that are larger or new in the problem part. Check whether substances such as crosslinker decomposition products like acetophenone, amines, antioxidant breakdown products, or siloxanes that can come from release agents appear, and trace back the raw materials and process steps through which each could enter. Moulding the same part without release agent, or retesting after wiping the surface, separates what comes from the surface from what comes from within.

Once the substance is known, agree with the raw material supplier whether to switch that additive to a grade with fewer odorous decomposition products or to reduce its amount. If release agent left on the surface is the cause, reset the release agent type and amount applied, and consider washing the surface after moulding. When changing an additive, confirm by testing whether other properties, such as cure rate and ageing performance, change with it.

Finding the cause

There is no need to send all five hypotheses to the lab at once. Rule them out starting with what records can confirm. Formulation and raw material lot changes, weighing records, cure conditions, and storage and transport history can all be checked at a desk. In-plant tests such as the curemeter and heating loss come next, and thermal desorption analysis and fogging and odour tests by the customer's method come last.

The first clue is when the problem began and where it clusters. If it appeared in every part from the moment a raw material or the compound changed, suspect light oil or a higher oil level; if it clusters in parts from one cavity or curing section, under-cure; if with the same compound only the summer shipments failed, storage temperature. If people say the character of the odour has changed, look at other additives such as crosslinkers, catalysts and release agents.

The shape of the symptom also separates the hypotheses. A heavy, oily film on the glass with a high condensate weight points to plenty of semi-volatiles such as oil and plasticiser, while odour alone with fogging within limits points to lower-boiling decomposition products or odorous substances such as amines. In thermal desorption analysis, a row of alkanes in the fogging range points to oil, and a few standout compounds point to the additive that produced them.

If that still does not settle it, run control trials that change one thing at a time. Make test pieces from the same compound with only the oil returned to the old grade, only the oil level lowered, only the cure time lengthened, or only the release agent left out, put them all through the same storage conditions, and measure fogging and odour the same way. Change only one thing at a time, or there is no telling which worked, and the job is done only when results pass the customer's test method with a comfortable margin.

The hypotheses can overlap. When a part loaded with light oil goes through a summer warehouse under-cured, the three causes feed one another: a loosely knit network holds the oil less firmly, and heat drives it out faster. In such cases, put the material side right first, meaning oil type and level and the state of cure, and deal with storage after that, because while the material holds plenty to emit, changing storage has little effect and results swing with the season, which makes them hard to judge.

Limits and cautions

Pass limits for fogging and odour, and test temperatures and times, differ by customer and method, so judgements follow the specification the customer names and its test conditions, and the volatile content and recommended cure of each raw material follow its TDS. Use in-plant heating loss or odour checks to narrow the cause, and decide pass or fail on results from an accredited laboratory. Changing the compound or a raw material can change physical properties and durability too, so take the part back through approval.

Safety matters too. Store peroxide crosslinkers, amine catalysts, process oils and plasticisers according to each product's safety data sheet, the SDS, and follow its guidance on protective equipment and ventilation. Extract fumes from post-cure ovens and heating tests, and for sniff tests keep to the set assessment procedure and sample size and avoid long sessions in enclosed spaces. Check flammability and inhalation hazards of solvents used for extraction in their SDS.

Sources

  1. Coran, A. Y. (1994). Vulcanization. In J. E. Mark, B. Erman, & F. R. Eirich (Eds.), Science and technology of rubber (2nd ed., pp. 339–385). Academic Press. https://doi.org/10.1016/B978-0-08-051667-7.50012-3
  2. Deutsches Institut für Normung [DIN]. (2011). DIN 75201:2011-11, Determination of the fogging characteristics of trim materials in the interior of automobiles. Superseded by the June 2024 edition. https://www.dinmedia.de/en/standard/din-75201/144385173
  3. International Organization for Standardization [ISO]. (2018). ISO 6502-3:2018, Rubber — Measurement of vulcanization characteristics using curemeters — Part 3: Rotorless curemeter. Withdrawn 2023. https://www.iso.org/standard/70969.html
  4. International Organization for Standardization [ISO]. (2021). ISO 6452:2021, Rubber- or plastics-coated fabrics — Determination of fogging characteristics of trim materials in the interior of automobiles. https://www.iso.org/standard/77554.html
  5. Liang, Y., & Xu, Y. (2014). Emission of phthalates and phthalate alternatives from vinyl flooring and crib mattress covers: The influence of temperature. Environmental Science & Technology, 48(24), 14228–14237. https://doi.org/10.1021/es504801x
  6. Minig, M., Reglitz, K., & Steinhaus, M. (2024). Odor-active compounds in flexible polyurethane materials. Indoor Air, 2024, 2415739. https://doi.org/10.1155/2024/2415739
  7. Nakamura, T. (2006). Organic peroxides as crosslinking agents. Nippon Gomu Kyokaishi, 79(6), 298–303. https://doi.org/10.2324/gomu.79.298
  8. Verband der Automobilindustrie [VDA]. (2011). VDA 278: Thermal desorption analysis of organic emissions for the characterization of non-metallic materials for automobiles.
  9. Verband der Automobilindustrie [VDA]. (2022). VDA 270: Determination of the odour characteristics of trim materials in motor vehicles. https://webshop.vda.de/VDA/en/vda-270-052022
  10. Wadey, B. L., & Holzmann, J. (1987). Plasticizers for automotive interior trim (SAE Technical Paper 870318). SAE International. https://doi.org/10.4271/870318
  11. Xu, Y., & Little, J. C. (2006). Predicting emissions of SVOCs from polymeric materials and their interaction with airborne particles. Environmental Science & Technology, 40(2), 456–461. https://doi.org/10.1021/es051517j
  12. Yoshida, T., & Matsunaga, I. (2006). A case study on identification of airborne organic compounds and time courses of their concentrations in the cabin of a new car for private use. Environment International, 32(1), 58–79. https://doi.org/10.1016/j.envint.2005.04.009

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.