Suspecting the die steel or its heat treatment is the usual response when hot forging dies crack or wear early, but these dies also answer to the lubricant sprayed between blows and to die temperature, so unless those are checked a new die tends to go the same way. What actually lies behind early failure can be uneven spray, wrong dilution, too little preheat, overcooling by spray or a film that will not stick, and sometimes two or more at once.

Background

A forging press that has been running blow after blow starts to leave corners underfilled and rough marks on the surface. With the die pulled, the cavity floor shows a spreading network of fine cracks like crazed glaze, and the convex corners have worn round and out of size. Changing the die means stopping the press and heating a new one, and parts forged in the meantime have to be sorted for size. A large crack that opens suddenly can throw die fragments and injure someone.

The loss does not stop at the price of the die. One analysis puts dies at 10 to 30% of the total cost of a forged part (Vianello et al., 2020); shorter die life can raise production cost by up to 40%, and 70% of dies withdrawn are withdrawn for plastic deformation or wear (Ficak et al., 2024). Dies fail in four ways: wear, mechanical fatigue and gross cracking, plastic deformation, and thermal fatigue cracking. Several of these run at once, but one of them usually ends the die's life (Uddeholm, 2017).

The graphite lubricant sprayed between blows, often called die release agent on the floor, does two jobs at once. When a suspension of fine graphite in water hits the hot die, the water evaporates and the graphite stays behind as a thin film that cuts friction and wear, while the evaporation draws heat out of the die surface (Mendez et al., n.d.). How much film stays and how far the die cools both depend on the spray conditions and the die temperature, so the same die steel can last very differently under different lubrication. One research group reported that after fitting a device that delivers a fixed lubricant dose at a fixed interval in an industrial process, die life doubled from 8,000 to 16,000 forgings (Hawryluk et al., 2023).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: do not scrap the damaged die straight away, photograph where it cracked and wore, and compare the number of parts it made and the dilution, spray time and die temperature records of the time with the lubricant's technical data sheet, the TDS.

Hypothesis 1: uneven spray

Look at this hypothesis first when the die shape changed with a new part number but nozzle position and angle did not, when the cavity has deep ribs or narrow grooves, when spray time was cut to shorten the cycle, or when a manually sprayed line gets a different amount from each operator. Picture a line where a new die with deep ribs went in but the nozzles stayed where they were for the previous part. Right after spraying, the broad floor of the cavity is covered in a grey film, while inside the ribs and on the corner far from the nozzle the metal still shows bright.

The graphite film keeps the hot workpiece from touching the die directly. In one set of experiments, friction rose when the graphite left on the die fell below a certain amount, and more than that brought no further gain (Mendez et al., n.d.). The same study explains that the amount that sticks is tied to how the spray cools the die, so it varies with spray time, the volume of liquid sprayed and whether a spot lies at the centre or the edge of the spray pattern, and that spraying more liquid can even leave less graphite behind. Where the film is short, the workpiece and its oxide scale slide over the die face under high pressure and wear it away, most markedly at convex radii and in the flash land (Uddeholm, 2017). Reviews also note that spray angle and direction decide whether the die wears evenly (Ficak et al., 2024).

Stop the press briefly after a spray, see where and how the graphite film covers the die, and photograph it. Catching the output of each nozzle in a container for the same time shows up blocked or weakened nozzles; laboratory work measures spray rate the same way, with a container held in front of the nozzle for a set time (Mendez et al., n.d.). Check nozzle angle, distance and spray time settings against the record from when the die was first set. Lay the worn and cracked areas over the areas where the film was thin, and it becomes clear whether the spray is to blame.

Where gaps in the film coincide with damage, reset the nozzles first. Fix nozzle position and angle for each die and keep them in a jig or a program, and add a nozzle or change its direction for deep cavities. Rather than adding spray by feel, consider automatic spraying that delivers a set amount every cycle. Devices that deliver a fixed dose at a fixed interval have been reported to make working conditions more repeatable and stable (Hawryluk et al., 2023).

Hypothesis 2: wrong dilution

Suspect the dilution when concentrate and water are mixed by eye, when an automatic mixer drifts off ratio, when the tank is topped up with water only, or when a tank left standing without stirring is started again. Graphite is heavier than water and settles when left still, so the top and bottom of the same tank can differ in strength. Take a line that runs its lubricant tank on Monday morning exactly as it stood over the weekend. Over the day the spray marks turn lighter and then darker, and by afternoon black residue begins to build up in the corners of the cavity.

The dilution ratio sets how much graphite a given volume of liquid carries. The die cools while graphite is sticking to it, so trying to build a thicker film by spraying more liquid tends only to chill the die further. Raising the share of graphite in the liquid is therefore put forward as the way to leave more graphite with less cooling (Mendez et al., n.d.). A lean mix pays the same cooling and leaves less film, and an over-rich one builds up as residue in the cavity. Reviews also note that a wrong balance between lubricant and coolant can contribute to micro-cracks and underfilled areas (Ficak et al., 2024). Suppliers give different dilution ranges for each process: the sheet for one water-based graphite lubricant recommends 5 to 10 parts water to 1 part concentrate for die forging and 2 to 10 for hammer forging, while stating that the right ratio has to be found in a trial on site and that the dilution should be stirred continuously so it does not settle (FUCHS, n.d.).

Measure concentration instead of judging it by eye. Take samples from the top and bottom of the tank and from a nozzle tip, dry a set amount of each, and compare the weight of solids left. Laboratory work measures the weight fraction of graphite in the suspension the same way, by evaporation (Mendez et al., n.d.). On lines with a mixer, measure the actual flows of concentrate and water and see whether they match the set ratio, and look in the top-up records for days when only water went in. If the same die shows both built-up residue and bare patches, suspect dilution and stirring together.

If dilution looks like the cause, fix the mixing method first. Set the ratio with a proportional mixing pump or a measuring vessel, top up with diluted lubricant at the same ratio, and keep the tank stirred while it is in use. When changing the ratio, move one step at a time within the supplier's range and record the film's appearance and the die condition together. Write the ratio found this way into the work standard, so the same liquid goes out whatever the shift.

Hypothesis 3: too little preheat

Preheating becomes the question when work starts on a cold die: right after a die change, on the first run after a weekend or a long stop, or on a winter morning. The habit of warming only the surface with a torch and starting to forge at once under time pressure belongs here too. Say that on the morning of a die change, a burner warmed only the cavity surface briefly before the first billet went in. For the first few blows the sprayed liquid pools and runs off the die and the corners of the part underfill, and before long a crack shows at a corner of the cavity.

When a red-hot billet meets a cold die, a large temperature difference opens between the surface and the interior all at once. A die steel supplier's guide lists inadequate preheating among the causes of gross cracking, alongside overload, design such as sharp radii, and excessive hardness, and states that proper preheating considerably reduces the risk of catastrophic failure by cracking (Uddeholm, 2017). Impact failure of hot forging dies has been reported to start frequently from surface cracks formed by mechanical or thermal fatigue (Ebara & Kubota, 1986). A cold die is also bad for lubrication. Below roughly the boiling point of water the liquid cannot evaporate fully, so it runs over the die and washes off graphite that has already stuck, and a die that is too cold chills the workpiece surface so that it flows poorly (Mendez et al., n.d.).

Measure die temperature at several points before the first blow. Use a contact thermometer not only on the cavity surface but at corners and thick sections, and record the preheating method and time and the temperature at the first blow. In a thermal fatigue study of forging dies, the upper and lower dies were preheated to 250 °C before work to avoid thermal shock (Vianello et al., 2020). If cracks tend to be found right after die changes or on the first run after long stops, the weight shifts towards preheating.

Put preheating into a written procedure so it does not vary with the person or the day. Take the target temperature from the ranges given by the die steel supplier and the lubricant TDS, and use a heating method and time that warm the whole die evenly rather than a torch that heats only the surface. Do not start spraying or forging before the target is reached, and reheat by the same procedure after long stops. Check the first few parts separately until the temperature has settled.

Hypothesis 4: overcooling by spray

This hypothesis belongs to lines where spray time was lengthened or a water spray added because the die was running hot, to the period just after a change to a water-based lubricant that cools more strongly, and to processes with a wide temperature swing in each cycle, such as press forging with long contact. Think of a summer afternoon when the die heated up and the operator lengthened the spray time a few times. Each spray sends up a large cloud of steam, and just before the next billet goes in the infrared thermometer reads lower than it did in the morning.

The die surface heats and cools every cycle. One forging die study explains that the surface, preheated to 250 to 300 °C, is heated by a billet at 950 to 1,200 °C and then cooled again by the lubricant spray, that this cycle causes thermal fatigue, and that its severity is set by the temperature difference, the peak temperature and the heating and cooling rates. In work the same study cites, thermal fatigue cracks began within less than 1% of die life (Vianello et al., 2020). A surface heated and cooled rapidly over and over develops a network of fine cracks, and raising the peak cycle temperature from 700 to 850 °C made the cracks grow roughly ten times faster (Persson, 2004).

The longer the spray, the further this swing reaches downwards. In simulations of multi-stage hot forging, lengthening the spray from 1.1 to 1.4 seconds lowered the peak die temperature by 13% (Veiga-Piñeiro et al., 2025), and the more the die cools, the further it climbs again at the next blow. A die steel supplier lists too hot a cavity surface, excessive cooling between forgings and inadequate preheating as conditions that increase thermal fatigue, all of them by widening the gap between the highest and lowest surface temperatures. Its guide adds that water-based lubricants cool the die more and raise the risk of thermal fatigue cracking, and that press dies, whose surfaces run hotter, can heat check early if lubrication chills them too much (Uddeholm, 2017).

Measuring the temperature swing is the starting point. At the same spot, take the surface temperature just after the part leaves, just after spraying ends and just before the next billet goes in, with an infrared thermometer or a surface thermocouple, and set the values before and after any change in spray time side by side. An infrared thermometer reads a graphite-coated surface differently from bare metal, so measure the same spot the same way each time. Look at the shape of the damage as well. A spreading network of fine cracks rather than one large crack, in the parts of the cavity that get hottest such as the floor or bosses, points to thermal fatigue.

The remedy is to cut the spray to what is needed to leave a film and treat cooling as a separate matter. Shorten the spray step by step to find the shortest time that still leaves an even film, and if cracking rose after a change to water-based lubricant, rework the dilution and spray time. If the die really is too hot, look at the cycle, billet temperature and contact time together before adding spray. The aim is a surface temperature that rises and falls within the same band every cycle.

Hypothesis 5: film will not stick

A film may fail to stick when a higher production rate leaves the die less time to cool, in processes with long contact, on a die covered with oxide or old residue, or with a lubricant whose working temperature range does not fit. Watch the spray up close on the day the production rate went up a step: the liquid clearly reaches the die, yet droplets bounce off and scatter as steam. Once the spray stops, the die face carries only a patchy film.

A water droplet that lands on a very hot surface boils at its underside first, makes a vapour layer and slides about on top of it. The temperature at which liquid stops wetting the surface and starts to float on a vapour film is the Leidenfrost point; at and above it, a vapour layer forms between liquid and solid almost at once, and the point shifts not only with the liquid's properties but with surface roughness and contamination (Bernardin & Mudawar, 1999, 2004). The vapour film also insulates the surface and weakens cooling (Veiga-Piñeiro et al., 2025).

The same thing happens with graphite lubricant. One study showed in experiments that while the die surface is hotter than the temperature at which graphite starts to stick, the spray only cools the die and the graphite disperses into the air, and film builds up only after the surface has cooled to that temperature. In the same study only 10 to 40% of the graphite sprayed stayed on the die, less on hotter dies, and the sticking temperature was about 264 °C under its test conditions, expected to vary with the carrier liquid, droplet size and velocity, and surface roughness and oxides (Mendez et al., n.d.). In tests gathered by one review, water-based lubricants adhered properly at 150 to 350 °C and oil-based ones at 250 to 850 °C, so the usable die temperature range differed by lubricant type (Ficak et al., 2024). A die that runs too hot has more than a film problem. Hot work die steel tempers further and softens the longer it stays at high temperature, and this softening is assessed with a tempering parameter that combines time and temperature (Virtanen et al., 2013).

The number to get first is the die surface temperature at the moment of spraying. Compare it with the working temperature range in the TDS, and photograph whether the film covers the die evenly after the spray. Spraying the same lubricant onto test pieces heated to set temperatures gives a rough idea, on the shop floor, of the temperature from which a film stays. Check as well whether a thick layer of oxide or burnt residue sits on the die surface and whether any area has visibly softened or sunk.

If high surface temperature is why the film will not stick, first bring the temperature at which the lubricant arrives into the range where it sticks. One proposal is a two-stage spray: cool with water first to bring the surface near the sticking temperature, then spray the lubricant (Mendez et al., n.d.). Decide with the supplier, by trial, whether a lubricant type with a higher working temperature is needed, and set nozzle distance and atomisation in the same trial. Remove oxide and residue at a fixed interval to keep the surface condition even.

Finding the cause

There is no need to investigate all five at once. Rule out first what can be measured without a long stop. Tank concentration and the output of each nozzle can be measured at once with a sample and a container, and die surface temperature with a thermometer during the cycle. Preheating records and die change history are already on paper. Taking the die down to examine the damage in detail comes after that.

The location and shape of the damage are the next clues. Wear at convex radii and the flash land, where the film was missing, points to spray distribution and dilution. A spreading network of fine cracks points to the heating and cooling swing, meaning overcooling or a surface running too hot. A single large crack that appeared just after a die change or near the first run points to preheating, and a patchy film with bouncing droplets on a softened surface points to a film that will not stick and a high surface temperature.

If that still does not settle it, run control trials that change one thing at a time. Correct only the nozzle angle, then switch to liquid freshly mixed at the set ratio, then shorten only the spray time. Change one thing at a time, or there is no telling which one worked, and with each change record photographs of the film and the surface temperature the same way.

The final check is the number of parts a die makes. Under the changed conditions, count die life on the same basis as before, such as parts made before regrinding or replacement, and see whether the damage pattern has changed. The job is done only when the life of a full die set has recovered, not the results of a few hours.

The hypotheses are bound up with each other. More spray cools the die further and raises thermal fatigue, less spray leaves too little film and raises wear, and a die that is too hot will not take a film however much is sprayed. A lean dilution lengthens the spray needed for the same film, and the die cools that much more. In such cases, first set the surface temperature at the moment of spraying inside the range where the film sticks, then adjust dilution and spray amount on that basis, because while the temperature is unsettled the effect of changing anything else cannot be compared fairly.

Limits and cautions

Suitable dilution, spray time, preheat temperature and die surface temperature differ by die steel, part shape, press and lubricant, so numeric decisions follow the lubricant's TDS and the die steel supplier's guidance. Whether a cracked die stays in service, is repaired by welding or is reground is for the die designer and a heat treatment specialist to decide, and a die with a visible large crack should not be kept running on floor judgement alone.

Safety matters too. Handle the lubricant with the protective equipment set out in the product's safety data sheet, the SDS. Breathing in graphite dust can cause respiratory symptoms such as cough, breathlessness and reduced lung function, so extract the spray mist so it does not spread, and clear dry residue from the tank and its surroundings without raising dust (NIOSH, n.d.). Inspect the die or fix nozzles only with the press stopped and locked out, and wear heat-resistant gloves and eye protection around preheated dies and burners.

Sources

  1. Bernardin, J. D., & Mudawar, I. (1999). The Leidenfrost point: Experimental study and assessment of existing models. Journal of Heat Transfer, 121(4), 894–903. https://doi.org/10.1115/1.2826080
  2. Bernardin, J. D., & Mudawar, I. (2004). A Leidenfrost point model for impinging droplets and sprays. Journal of Heat Transfer, 126(2), 272–278. https://doi.org/10.1115/1.1652045
  3. Ebara, R., & Kubota, K. (1986). Failure analysis of hot forging dies. In Steel forgings (pp. 583–592). ASTM International. https://doi.org/10.1520/STP17381S
  4. Ficak, G., Łukaszek-Sołek, A., & Hawryluk, M. (2024). Durability of forging tools used in the hot closed die forging process—A review. Materials, 17(22), 5407. https://doi.org/10.3390/ma17225407
  5. FUCHS. (n.d.). LUBRODAL F 24 W [Product information]. Retrieved November 2026. https://www.fuchs.com/de/en/product/product/148408-LUBRODAL-F-24-W/
  6. Hawryluk, M., Dudkiewicz, Ł., Marzec, J., Rychlik, M., & Tkocz, R. (2023). Selected aspects of lubrication in die forging processes at elevated temperatures—A review. Lubricants, 11(5), 206. https://doi.org/10.3390/lubricants11050206
  7. Mendez, P. F., Castro, G., & Martinez, F. (n.d.). Influence of heat transfer on the application of solid lubricant on hot dies [Author manuscript]. Colorado School of Mines. Retrieved November 2026. https://sites.ualberta.ca/~pmendez/Publications/Papers/2007_jopd_lubricant.pdf
  8. National Institute for Occupational Safety and Health [NIOSH]. (n.d.). NIOSH pocket guide to chemical hazards: Graphite (synthetic). Centers for Disease Control and Prevention. Retrieved November 2026. https://www.cdc.gov/niosh/npg/npgd0307.html
  9. Persson, A. (2004). Strain-based approach to crack growth and thermal fatigue life of hot work tool steels. Scandinavian Journal of Metallurgy, 33(1), 53–64. https://doi.org/10.1111/j.1600-0692.2004.00678.x
  10. Uddeholm. (2017). Uddeholm tool steels for forging applications (Edition 4). Uddeholms AB. https://voestalpine.com/highperformancemetals/schweiz/fr/uddeholm_schmieden_en
  11. Veiga-Piñeiro, G., Martin-Ortega, E., & Pérez-Betanzos, S. (2025). Thermal management in multi-stage hot forging: Computational advances in contact and spray-cooling modelling. Materials, 18(14), 3318. https://doi.org/10.3390/ma18143318
  12. Vianello, P. I., dos Santos, A. J., Abrão, A. M., & Magalhães, F. C. (2020). Thermal fatigue analysis of hot forging closed dies. Materials Research, 23(4), e20190697. https://doi.org/10.1590/1980-5373-MR-2019-0697
  13. Virtanen, E., Van Tyne, C. J., Levy, B. S., & Brada, G. (2013). The tempering parameter for evaluating softening of hot and warm forging die steels. Journal of Materials Processing Technology, 213(8), 1364–1369. https://doi.org/10.1016/j.jmatprotec.2013.03.003

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.