KALTECKOREA

BlogApplication notes

Why does water get into gearboxes and cause rust and pitting?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Equipment/Service Lubricants

Changing the oil is the usual response when water turns up in a gearbox, but if the way in stays open, the new oil takes on water again and the rust and pitting carry on. What actually lets it in can be wash water and rain getting past the seals, humid air drawn in through the breather, oil that separates water poorly, a leaking cooling coil or condensation while the unit stands idle, and sometimes two or more at once.

Background

Undo the drain plug of a gearbox and cloudy water runs out before the oil. Open the inspection cover and the gear teeth show red rust stains and small pits, while a rough noise that was not there before comes from the bearings. A few weeks after an oil change the same picture returns, and in the end the line stops so that gears and bearings can be replaced.

Water cuts directly into the life of gears and bearings. In life tests of tapered roller bearings run with 25, 100 and 400 ppm of water in the oil, fatigue life fell in clear step with the water content (Cantley, 1977). In tests on bearing steel, micropitting and rolling contact fatigue increased whether the water was dissolved or free, while surface wear changed little (Qin & Doll, 2022). In running tests of case-carburised gears, water at 5,000 to 20,000 ppm generally lowered pitting load capacity, and undissolved water appeared more harmful than dissolved water (Engelhardt et al., 2017). The loss grows in stopped lines and replaced parts more than in the cost of the oil.

Water in oil is either dissolved, dispersed as fine droplets that turn the oil cloudy, or separated out as free water that collects at the bottom. Oil can hold only so much in solution, and water beyond that limit separates as free water (Al Sheikh Omar et al., 2024). So how close the water is to that limit matters as much as its amount, and the researchers behind the gear tests proposed the oil's relative humidity, with 100% as the threshold, as the yardstick (Engelhardt et al., 2017). Hard steels such as bearing steel resist corrosion poorly, so water in contact with them makes rust, and that spot can later lead to fatigue starting at the surface (Rodriguez & Meyers, 2022).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: draw a drain sample into a clear bottle, see whether water separates at the bottom or the whole oil is cloudy, note when and where water showed up, and compare this with the oil's technical data sheet, the TDS, and with how the gearbox is installed and run.

Hypothesis 1: water past seals

Look at this hypothesis first where equipment is washed daily with hoses or pressure washers, as in food and beverage plants, on outdoor conveyors and pump drives exposed to rain, and on gearboxes mounted low enough for water to splash on them. A shaft seal is made to hold oil in, so when a jet of water strikes it from outside or water pools around it, its ability to keep water out has limits. Picture the night clean, with an operator walking under a conveyor and sweeping a pressure washer along it. The jet reaches the output shaft end and the seal around it, and the housing of the gearbox, just stopped, is still warm. The sample drawn the next morning is cloudier than the day before.

Water has two ways in. One is a hard jet forcing its way straight between seal lip and shaft; the other opens when a warm gearbox cools. As the air inside cools and contracts, the pressure inside falls below the pressure outside, and that difference draws water pooled around the seal inwards. This is why, when bearing makers assess seals, they heat a bearing to 100°C, plunge it straight into water at room temperature and weigh the water it took in, and run a separate test washing it with hot water at over 100 bar (SKF, 2003). Water that gets in this way is heavier than oil, so it sinks, and the lowest bearings and gears are the first to sit in it.

The thing to establish is when the water rises. Sampling at the same point before a wash, the day after a wash and the day after rain shows the pattern. Measured by Karl Fischer titration, a standard method, the water content comes out as a number that includes dissolved water (ASTM International, 2025). Check the shaft around the seal for a rust band or water marks, and the seal lip for cracks and the shaft for a groove. Do not skip watching the wash itself to see from which direction the water reaches the seal.

With washing shown to be the cause, keep the jet off the seals first. Fit covers or splash guards over seals and shaft ends, add a line to the cleaning instructions not to aim directly at gearbox shaft ends, and change the order of work so that cold water is not sprayed straight onto a hot gearbox. Replace worn seals, and where water strikes often, review with the gearbox maker a seal with an extra outer dust lip. After washing, drain the free water from the bottom.

Hypothesis 2: humid breather air

A gearbox warms as it runs and cools when it stops, so each time it breathes air out through the breather and draws it back in. Check whether this breathing carries water where the air is humid, as in the rainy season, by the sea or in plants full of steam and mist, on outdoor equipment with wide swings between day and night, and on machines that start and stop often. Take an outdoor gearbox with an open-cap breather through a week of steady rain. It runs by day and stands at night, and droplets sit on the underside of the inspection cover.

Water vapour in the air drawn in turns to water when it meets a cold wall. Air cooled below its dew point cannot hold all its vapour, and the surplus condenses on the inner walls and cover and runs down into the oil. Research on wind turbine gear oils also notes that water can condense inside the gear housing, contaminate the lubricant and shorten component life (Tobie et al., 2012). Water that enters a little at a time stays dissolved and unseen at first, and the harm grows as the oil nears the limit of what it can hold. In case-carburised gear tests at lower water contents of 1,000 to 2,900 ppm, an effect on pitting load capacity appeared only when the oil's relative humidity was above 100% (Engelhardt et al., 2017).

The clue is where the rust has formed. Rust on the inside of the housing top above the oil, on the back of the cover or below the breather points to water condensed from the air. See what kind of breather is fitted and, if it holds desiccant, whether the colour has fully changed. Log the water content alongside season, weather and operating pattern, and it shows whether it creeps up with humid seasons and frequent stops. A moisture sensor that reads the oil's relative humidity directly shows when it crosses the line.

If breathing is the cause, dry the air that goes in. Replace an open breather with one that holds desiccant, and change the desiccant before its colour turns. Move the breather, or shield it, so that wash jets and rain do not hit it directly. In very wet places, review with the gearbox maker a breather designed to draw in less outside air as the temperature changes.

Hypothesis 3: poor demulsibility

Some water getting in is hard to avoid on many sites. What matters then is how fast the oil separates that water and sends it to the bottom, a property called demulsibility. Consider it when the oil has been in service long enough to oxidise, when a different oil has been used for top-up, when cleaning agents have got in, or when the oil in the gearbox is not one meant for it. Suppose two gearboxes on the same line are washed the same way. Open the drain on one and a little clear water comes out ahead of the oil; on the other, the whole charge is milky.

When oil separates water well, droplets merge and settle, and the water gathered at the bottom can be drained. When it separates poorly, the water stays spread through the oil as fine droplets and keeps being carried into the contacts of gears and bearings. The researchers behind the gear tests named breakdown of additives and faster ageing of the oil as the main routes of water damage (Engelhardt et al., 2017). In engine oil tests too, water used up additives, and lubricating performance did not fully return even after free water was removed (Al Sheikh Omar et al., 2024). In one study, the more water was dissolved, the thinner the protective film formed by additives and the more micropitting began (Soltanahmadi et al., 2017).

The simplest check is to stand a sample in a clear bottle somewhere warm and see how long the water takes to separate at the bottom. Doing the same with new oil and setting the two side by side makes the difference plainer. In the laboratory, the standard test for demulsibility of medium and higher-viscosity lubricants such as gear oils mixes oil and water, then measures the separated water, the emulsion layer and the oil (ASTM International, 2022). Compare the result with the value for new oil or the TDS, and check the top-up records for any other oil mixed in.

Oil that has lost its ability to separate water does not recover by draining alone, so change it. If mixed oil or a cleaning agent is to blame, flush the gearbox before refilling, and where water gets in often, choose with the supplier a gear oil with a specified demulsibility result. Label top-up containers so that only the same oil goes in. Good separation only makes water easier to drain, though, so the way the water gets in still has to be found and closed.

Hypothesis 4: leaking cooling coil

Some large gearboxes have a coil carrying cooling water inside the sump, or an external oil cooler cooled by water. On such units, suspect the coil when the water content has jumped, when the cooler is old, when cooling water treatment has been lax, or when the cooling water has ever frozen in winter. Think of a gearbox stopped over the weekend with the cooling water valve left open. On Monday morning the sight glass reads higher than it did on Friday.

The coil in the sump carries cooling water under pressure, while the oil around it is close to atmospheric pressure. So even a pinhole lets water push out into the oil along that pressure difference, and it keeps coming in for as long as cooling water flows, even with the gearbox stopped. Tubes are holed in several ways. In a study of leaking brass tubes from a lubricating oil cooler, stress corrosion cracks started from small pits left where zinc had leached out of the alloy (Qu et al., 2011). Water entering this way, unlike water condensed from air, comes in quantity, so it can raise the oil level and quickly emulsify the whole charge.

The oil level record is the first clue. A level that rises with no oil added means liquid has come in from outside. Run for a few days with the cooling water shut off to see whether the water content stops climbing, and at a shutdown, remove or blank the coil and pressure-test it to see whether the pressure drops. If the cooling water carries treatment chemicals, their elements turning up in oil analysis are another clue. See as well whether the cooling water outlet temperature behaves differently from usual.

Once a leaking coil is confirmed, shut off its cooling water until it is repaired or replaced, drain the water from the oil and judge from its condition whether to change it. Add a step that closes the cooling water whenever the gearbox is stopped, so that water has no time to get in while it stands. To stop a repeat, set a standard for cooling water treatment, and drain units standing idle in winter so they cannot freeze. Confirm with the gearbox or cooler maker that the tube material suits the cooling water.

Hypothesis 5: condensation at rest

Standby gearboxes, seasonal equipment, lines stopped for long holidays and machines in unheated buildings, water forms and pools while the unit stands. While running, the oil is warm and holds more water in solution, and as it cools at rest it gives that water up. A standby pump gearbox that has stood all summer is started for the first time in autumn. The bearings sound rough as it starts, and the bearing raceways, once removed, show rust marks lined up at even intervals.

Water at rest comes from two places. Water the cooled oil can no longer hold separates out, and when the housing walls follow the night air below the dew point, vapour in the air inside condenses on them. Water beyond what the oil can hold becomes free water, and in gear tests undissolved water appeared more harmful than dissolved water, so the same amount of water can do more harm in cold oil (Engelhardt et al., 2017). In a bearing that is not turning, that water stays where rolling elements meet the raceway. The rolling bearing damage classification calls this moisture corrosion: with the bearing at a standstill, the raceway is damaged at the spacing of the rolling elements, and on restart those spots can lead to fatigue starting at the surface (ISO, 2017; Rodriguez & Meyers, 2022). One view holds that undissolved water may also raise the risk of early pitting through cracking in which hydrogen plays a part (Tobie et al., 2012).

Lay the symptoms over the shutdown record. Check whether water and rust cluster after long stops or cold seasons, and appear less on the same model that runs continuously. If a bearing can be removed, see whether the spacing of the rust marks matches that of the rolling elements. Draw one sample from the bottom just before restart and another after a good run, and comparing their water content shows how much separated out and pooled during the stop.

To cut condensation at rest, start with the equipment that will stand longest. Run standby units briefly at set intervals or turn the shaft by hand so the rolling elements do not rest in the same place, and fit a desiccant breather so the air drawn in as they cool is dry. Before restart, drain the free water from the bottom first. For equipment going into long storage, follow the gearbox maker's storage instructions for oil fill and rust protection.

Finding the cause

There is no need to search all five at once. Start with what is already to hand: a sample bottle, the oil level record, and the operating and cleaning logs. If water separates clearly at the bottom of a standing sample, concentrate on finding the way in; if the whole oil stays cloudy for a long time, suspect the oil's ability to separate water as well. Record the water content as a Karl Fischer number so that the effect of any later change can be compared (ASTM International, 2025).

Next come the amount of water and when it arrives. Enough water to raise the level with no top-up points to a route that lets liquid straight in, such as the cooling coil or wash water. A rise the day after washing or rain points to water past the seals, and one that stops when the cooling water is shut off points to the coil. Small amounts climbing steadily through humid seasons point to humid air through the breather, and water pooling after long stops or cold nights points to condensation at rest.

Where the rust sits points the way too. Rust on the inside of the top and the back of the cover, above the oil, comes from water condensed out of the air, while rust gathered on the shaft by the seal and on the lowest bearings marks where water from outside settled. Rust lined up on a raceway at the spacing of the rolling elements is read as water that sat there while the bearing stood still (ISO, 2017).

If that still does not settle it, run control trials that change one thing at a time. Wash for a few weeks with seals and shaft ends covered, or swap only the breather for a desiccant type, or run with the cooling water shut off. For each trial, sample at the same point under the same conditions and compare the water content with that before the change. Only when it stays low after a single change is that route closed.

The hypotheses often overlap. When wash water cools a warm gearbox, water past the seals and humid air drawn through the breather both rise, and a long stop lets that water pool at the bottom. If the oil separates water poorly, water from any route lingers longer in the contacts. In such cases, close the routes that let liquid straight in first, then cut the moisture from air and from standing, and change to fresh oil that separates water well last. Change the oil before the water is stopped, and the new oil takes on the same water again.

Limits and cautions

Acceptable water levels, demulsibility limits, breather types and storage methods differ by oil, gearbox and duty, so numeric decisions follow the oil's TDS and the gearbox maker's instructions. Compare laboratory water and demulsibility results only with results from the same method and the same sampling point. Gears already pitted and bearings already rusted do not recover once the water is stopped, so whether they can stay in service is for the gearbox maker or a maintenance specialist to judge from vibration readings and a teardown inspection.

Take samples or open the drain only with the gearbox stopped and locked out. Oil in a gearbox that has just stopped is hot enough to burn, and pressure can remain inside the housing, so open breathers and plugs slowly. Wipe up spilt oil and water at once because they are slippery, and for oils, cleaning agents and desiccants, follow the product's safety data sheet, the SDS, for protective equipment and disposal.

Sources

  1. Al Sheikh Omar, A., Salehi, F. M., Farooq, U., & Morina, A. (2024). Additives depletion by water contamination and its influences on engine oil performance. Tribology Letters, 72(3), 74. https://doi.org/10.1007/s11249-024-01876-y
  2. ASTM International. (2022). ASTM D2711-22, Standard test method for demulsibility characteristics of lubricating oils. https://store.astm.org/d2711-22.html
  3. ASTM International. (2025). ASTM D6304-25, Standard test method for determination of water in petroleum products, lubricating oils, and additives by coulometric Karl Fischer titration. https://store.astm.org/d6304-25.html
  4. Cantley, R. E. (1977). The effect of water in lubricating oil on bearing fatigue life. ASLE Transactions, 20(3), 244–248. https://doi.org/10.1080/05698197708982838
  5. Engelhardt, C., Witzig, J., Tobie, T., & Stahl, K. (2017). Influence of defined water contents in gear lubricants on the pitting performance of case-carburized gears. In Proceedings of the ASME 2017 International Power Transmission and Gearing Conference, Vol. 10, V010T11A037. https://doi.org/10.1115/DETC2017-67016
  6. International Organization for Standardization [ISO]. (2017). ISO 15243:2017, Rolling bearings — Damage and failures — Terms, characteristics and causes. https://www.iso.org/standard/59619.html
  7. Qin, H., & Doll, G. L. (2022). Effects of water contamination on micropitting and rolling contact fatigue of bearing steels. Journal of Tribology, 145(1), 011501. https://doi.org/10.1115/1.4055181
  8. Qu, S., Yao, G., Tian, J. F., & Zhang, Z. F. (2011). Failure analysis of the brass tubes in a lubricating oil cooler. Engineering Failure Analysis, 18(8), 2232–2239. https://doi.org/10.1016/j.engfailanal.2011.07.018
  9. Rodriguez, D., & Meyers, K. E. (2022). Bearing damage analysis: ISO 15243 is here to help you. SKF Evolution. Retrieved November 2026. https://evolution.skf.com/bearing-damage-analysis-iso-15243-is-here-to-help-you/
  10. SKF. (2003). New sealing solutions for deep groove ball bearings. SKF Evolution. Retrieved November 2026. https://evolution.skf.com/new-sealing-solutions-for-deep-groove-ball-bearings/
  11. Soltanahmadi, S., Morina, A., van Eijk, M. C. P., Nedelcu, I., & Neville, A. (2017). Tribochemical study of micropitting in tribocorrosive lubricated contacts: The influence of water and relative humidity. Tribology International, 107, 184–198. https://doi.org/10.1016/j.triboint.2016.11.031
  12. Tobie, T., Stahl, K., Höhn, B.-R., & Witzig, J. (2012). Effects of water in wind turbine oils on the gear load capacity. In Society of Tribologists and Lubrication Engineers Annual Meeting and Exhibition 2012 (pp. 459–461). STLE.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.