KALTECKOREA

BlogApplication notes

Why do generator bearings show electrical pitting?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Equipment/Service Lubricants

Replacing the bearing is the usual response to electrical pitting on a generator bearing, but unless both the path that drains shaft voltage and the oil film that has to withstand it are put right, the same marks tend to return on the new bearing. What actually lies behind them can be a worn earth brush, failed bearing insulation, a thin oil film, oil made conductive by water and oxidation, or carbon and metal debris left by discharges, and sometimes two or more at once.

Background

At a scheduled overhaul the generator bearing is opened, and one band of a rolling bearing raceway has turned a dull grey, or the face of a sleeve bearing is covered in tiny holes as if pricked with a needle. If vibration had been creeping up and bearing temperature wandering before that, these marks may have been where it started. Changing the bearing means stopping the generator, and an unplanned change costs lost generation, parts and labour. If the marks are found only after they have spread into a washboard pattern, the shaft journal may need work as well as the bearing.

These marks start with voltage on the shaft. A generator shaft picks up voltage from several sources, such as asymmetry in the magnetic circuit, a static excitation system and static charge building up on the rotor, and voltage from static excitation has been analysed separately in large turbine generators, with countermeasures tested (Ammann et al., 1988). Normally the thin oil film in the bearing blocks this voltage like an insulator, but when the voltage exceeds the film's dielectric strength the film breaks down, an arc jumps, and the metal at that spot melts for an instant, leaving a small crater (Puchtler et al., 2024). Such damage has been described in four forms, frosting that leaves a dull, misty surface, pitting, spark tracks along the direction of rotation and welding, and the international standard lists excessive current erosion and current leakage erosion as their own branch of rolling bearing damage (Costello, 1993; ISO, 2017).

So the cause is sought on two sides: whether the path that lets shaft voltage drain to earth without passing through the bearing has been blocked, and whether the oil film in the bearing has become too thin to withstand that voltage or has turned conductive. The first is a matter of earthing and insulation, the second of the lubricant, and fixing only one side lets marks return from the other. In other fields such as electric vehicle drives, too, research has built up on how shaft voltage and bearing current cause surface damage and lubrication failure together (He et al., 2020).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph which bearing carries the marks and on which side, take an oil sample before draining, and measure shaft voltage and earth current in operation, then compare them with the generator maker's limits and the oil's technical data sheet, the TDS.

Hypothesis 1: worn earth brush

One end of a generator shaft usually carries an earth brush that rides on the shaft and lets voltage drain to earth. Made of carbon or silver graphite, these brushes wear, glaze over and lose performance in damp or dirty surroundings, and cases have been reported where poor maintenance or low spring tension led to higher shaft voltage (Mailula & Saha, 2025). Look at this hypothesis first on generators with heavy oil mist around the brush holder, in dusty generator halls, and on sites with no set interval for brush checks.

Picture opening the brush holder to find the brush worn short inside it, the spring stretched almost to its limit, and the face that touches the shaft glossy black with oil and dust caked together. The brush track on the shaft is coated in a thin film of oily grime as well. There is no record of the brush being changed at the last overhaul.

Once the brush loses proper contact with the shaft, the easy path for shaft voltage is gone. When static charge builds on the rotor, shaft voltage climbs slowly in a sawtooth, then drops sharply the moment it reaches what the oil film can withstand and discharges through the bearing, and this repeated cycle is linked to discharge damage in bearings. The same review cites a case where an open-circuited earth brush let shaft potential rise until the bearing failed completely, and notes that brushes are sensitive to oil film, dust and misalignment (Mailula & Saha, 2025). One discharge leaves one small crater, but countless discharges together turn the whole surface misty, and this frosted surface is regarded as the stage before fluting, the washboard-like damage (Schneider et al., 2022).

Checking begins with the brush itself. Look at remaining length, spring tension, the condition of the contact face and any grime on the shaft track, and confirm continuity from the brush to earth with no broken or loose lead. In operation, measure shaft voltage and earth current and record the waveform. Measuring shaft voltage and current directly has been put forward as the most effective way to identify the voltage source, and continuous watching of shaft voltage and earth current through an insulated shaft-riding brush has been reported to catch problems early (Costello, 1993; Nippes, 2004). A sawtooth waveform points to static charge, and a waveform at line frequency and its multiples to magnetic asymmetry (Mailula & Saha, 2025).

If the brush is the cause, replacement and cleaning come first, and then keeping it from happening again. Clean the brush and its shaft track, and add a rule to the maintenance plan for changing the brush before it wears below a set length. Stopping oil mist that leaks towards the holder is part of the same job. Measuring shaft voltage and earth current the same way at every overhaul shows a weakening brush in the numbers before the next set of marks.

Hypothesis 2: failed insulation

Voltage from magnetic asymmetry tries to drive a current around a loop through shaft, bearings and frame, so large generators usually insulate one bearing, often at the non-drive end, to break that loop (Mailula & Saha, 2025). The insulation may be a plate under the bearing pedestal or a coating on the bearing itself. Look at this hypothesis after reassembly following an overhaul, when new piping or instrument cables have been run across the insulating plate, or when oil and dust have built up around the pedestal over years.

A few months after an overhaul, vibration starts to rise at both bearings. Opened up, not only the drive-end bearing but also the insulated non-drive-end bearing shows discharge tracks running in the direction of rotation. The work record shows that a temperature sensor cable was newly fixed to the non-drive-end pedestal during reassembly.

The insulation's job is to keep the loop broken at one point, so a single metal-to-metal link anywhere closes it again. A circulating current at line frequency then passes through both bearings, and over time it produces frosting or fluting on the raceways. Insulation can degrade gradually through thermal cycling, mechanical stress and contamination, and the reappearance of shaft voltage at the insulated end, or a sudden drop in the voltage difference, is read as a strong sign that the insulation has failed or been bypassed (Mailula & Saha, 2025). Once the loop is closed the current passes through both bearings, so marks on the insulated-end bearing mean the insulation is not doing its job.

Insulation is checked both running and stopped. In operation, measure the shaft-to-earth voltage at both ends and compare them; at standstill, measure the insulation resistance between pedestal and base across the insulating plate, using the method and voltage the maker specifies. Periodic insulation resistance tests combined with shaft earth current monitoring and a trend of shaft voltage are recommended (Mailula & Saha, 2025). If the reading is low, remove pipe flanges, bolts, cable clamps and built-up dirt that cross the plate one at a time to find where the link is.

Once the bypass is found, break it with an insulating bush or washer, and wipe the oil and dust from around the plate. If the plate or coating itself is damaged, plan its replacement at the next outage and measure shaft voltage more often until then. Add a step to the maintenance procedure to measure and record insulation resistance after reassembly, so the same thing does not happen again.

Hypothesis 3: thin oil film

Even with sound earthing and insulation, an oil film that is too thin lets discharges happen at lower voltage. Suspect this hypothesis when cooling water warms up in summer and the bearing oil runs hot, when a lower viscosity grade has been mixed in during top-up, when higher output has raised bearing load, or when frequent starts and stops mean long spells at low speed.

A midsummer afternoon: the bearing oil temperature is running above normal, and the label on the drum used for last month's top-up shows a viscosity grade one step lower than the usual oil. The shaft voltage reading is no different from the last overhaul.

How much voltage an oil film withstands depends on the minimum film thickness in operation and on the lubricant's electrical properties; as lubricant temperature rises, viscosity falls and the minimum film gets thinner, so the voltage at which discharge occurs also falls. Bearings have also been reported to pass current more easily once they have had a first breakdown (Puchtler et al., 2024). Higher load thins the film, and rotational speed also changes film thickness (Schneider et al., 2022). The closer the film comes to mixed friction, where it breaks between metal peaks, the more metal contacts there are and the easier it is for current to pass. A crater, once formed, roughens the surface and invites the next discharge, so a thin film quickly enlarges small damage.

This can be checked in numbers. Match bearing oil and cooling water temperature records against when the marks appeared, and measure the in-service oil's kinematic viscosity at 40 °C against the new-oil value in the TDS. Search the top-up records for any other viscosity grade or product, and check the operating records for changes in load and number of starts. On sets that share turbine oil, such as turbine generators, follow the test items and intervals in the in-service monitoring standard and watch the viscosity trend (ASTM International, 2024).

If viscosity has dropped, return to the grade the maker specifies, and mark drums and filler points so top-ups use only the same product. If high oil temperature is the cause, start by cleaning the cooler and restoring cooling water flow. Raising viscosity also changes friction heat and starting behaviour, though, so any change outside the specified grade is agreed with the generator maker.

Hypothesis 4: conductive oil

When oil ages and takes on water, it conducts better even at the same film thickness. Typical cases are a cooler that leaks water, an oil tank that breathes humid air and gathers condensation, and oil kept past its change interval until it has oxidised. It is all the more likely if marks increased after a rainy season or a run of large day-night temperature swings.

Stood by a window, the oil sample looks hazy where it should be clear, and a few droplets of water settle at the bottom of the bottle. The colour is clearly darker than last year's sample. Open the tank inspection cover and droplets have formed on the underside of the lid.

How well oil conducts is set by the concentration of ionic substances in it, and lubricants can become conductive because of additives or oxidation products (Iwase et al., 2024). When the same study oxidised a polyalphaolefin synthetic oil, the unoxidised oil showed no loss from conduction, while the oxidised oil rose in conductivity, acid number and viscosity together. In engine oil oxidised in the laboratory, too, water content, electrical conductivity, permittivity and acid number all rose with oxidation time, and organic acids from oxidation are described as reacting with water to form acidic substances, inorganic acids among them (Zhou et al., 2024). A conductive film cannot hold the voltage to the end, so discharges and leakage current can increase even at the same shaft voltage. A review of large generators likewise concludes that keeping the dielectric strength and cleanliness of bearing oil through filtration and good lubrication practice is key to reducing how often the oil film breaks down (Mailula & Saha, 2025).

Water and oxidation show up in oil analysis. Measure water with the standard Karl Fischer titration method, a standard that notes moisture can lead to premature corrosion and wear (ASTM International, 2025). Measure acid number, viscosity and appearance as well and compare them with new oil and the trend of past samples, and if the laboratory can measure electrical conductivity or dielectric properties, have those done too. Oil conductivity changes strongly with temperature, so compare only values measured at the same temperature. If water is found, trace how it got in with a cooler leak test and a look at the tank breather.

Water has to be stopped where it gets in first. Then dry the oil with a water removal unit or vacuum dehydration, or replace it depending on its condition. Oil whose acid number has risen sharply keeps its oxidation products even when dried, so consider replacing it. Fit a desiccant breather to the tank vent, and set an oil analysis interval so the point where water and acid number start to rise is not missed.

Hypothesis 5: discharge debris

In a bearing where electrical erosion has been going on for some time, the discharges change the oil itself. If the marks were found late, if only the bearing was changed and not the oil, or if marks are spreading to other bearings on the same oil system, it is time to suspect the oil. On smaller grease-lubricated generators, grease turning black in a short time is the same signal.

Take a generator that got a new bearing while its oil was filtered and put back. A few months later, the new bearing already shows a faint grey band, and oil mixed with fine black powder has pooled at the bottom of the bearing housing.

At the tiny contact spots where discharges pass, current density is very high and temperature rises sharply; the heat splits lubricant molecules and releases carbon, blackening the oil and weakening its lubrication. Metal oxide debris shed from the damage promotes oil oxidation and raises lubricant conductivity (Safdarzadeh et al., 2024). Oil carrying carbon and metal particles conducts better and roughens the film, so a loop can form in which discharges invite more discharges. Electrical load has been summarised as changing the lubricant's appearance and ageing it early, so that it lubricates less well (Schneider et al., 2022). In thrust bearing tests with a mineral oil, however, oil analyses such as infrared spectroscopy and viscosity showed no clear effect of the electrical load, even though the raceways had clear electrical damage (Graf et al., 2023). A clean oil analysis does not rule out discharges.

Look at oil and bearing together. Check the colour and amount of debris at the housing bottom and in the filter, and in the oil analysis follow the trend of wear metals such as iron, contamination level and acid number. A removed bearing is judged by the shape of its marks; the international standard classifies damage by appearance and calls for further work such as cross-sections when that is not enough (ISO, 2017). Settling under a microscope whether the craters show melting, or are plain corrosion pits or fatigue spalls, makes the next decision easier.

If discharge products have built up, do not change only the bearing; flush the oil system and replace the oil as well. Wash out black residue left in the housing and piping, and after filling with new oil, take samples at short intervals to see that iron and contamination do not climb again. Above all, the path of the voltage that caused the discharges has to be put right at the same time, or the new oil and new bearing will go the same way.

Finding the cause

There is no need to work through all five hypotheses at once. Rule things out starting with what can be seen without stopping. Measuring shaft voltage and earth current, checking the brush and analysing an oil sample can all be done in operation, while insulation resistance and bearing teardown wait for a stop.

The first fork is shaft voltage and its waveform. If shaft voltage is higher than usual or than the maker's limit, look first at why it cannot drain: the earth brush and the insulation. A sawtooth points to static charge and brush contact; a large line-frequency component with a shrinking voltage difference between the two ends points to bypassed insulation. If shaft voltage is unchanged yet marks appear, what the oil film can withstand has fallen, so move to the oil: viscosity, temperature, water and acid number.

Where the marks sit is a clue too. Marks on the insulated-end bearing as well point to circulating current and bypassed insulation; marks spread evenly over several bearings on one oil system point first to oil condition and discharge products. If the marks grew in a particular season, such as summer or after the rains, match temperature and water records to that period.

If that still does not settle it, change one thing at a time. Fit a new brush and clean its track, then see how shaft voltage and earth current respond; next break the insulation bypass; next dry or replace the oil. Changing everything at once leaves no way of telling what worked. The job is done when shaft voltage and earth current are stable, the bearing opened at the next overhaul has no new marks, and iron, water and acid number in the oil analysis stay flat.

Hypotheses can overlap. Discharges from a weakening brush leave carbon and metal particles in the oil, and that oil conducts better, so discharges increase at the same voltage. High oil temperature thins the film and speeds up oxidation too. In such cases, put the voltage path, the earthing and insulation, right first and then replace the oil, because changing the oil alone while the voltage stays leaves the new oil to build up discharge products again.

Limits and cautions

Allowable shaft voltage and earth current, insulation resistance limits, oil viscosity grade and change criteria differ by generator type, bearing type and oil, so numeric decisions follow the generator maker's limits and the oil's TDS. Measurements on the shaft, brush changes and insulation tests are done close to rotating parts and high voltage, so leave them to staff who know the generator's operating and electrical safety procedures, and carry out standstill work only after mechanical and electrical isolation and lockout. Decide on bearing damage and any journal repair together with the maker or a specialist service company.

When sampling or handling oil, wear protective gloves and safety glasses as the product's safety data sheet, the SDS, requires, and take care around hot oil and rotating parts. Dispose of filtered debris and used oil according to local regulations.

Sources

  1. Ammann, C., Reichert, K., Joho, R., & Posedel, Z. (1988). Shaft voltages in generators with static excitation systems: Problems and solution. IEEE Transactions on Energy Conversion, 3(2), 409–419. https://doi.org/10.1109/60.4749
  2. ASTM International. (2024). ASTM D4378-24, Standard practice for in-service monitoring of mineral turbine oils for steam, gas, and combined cycle turbines. https://store.astm.org/d4378-24.html
  3. ASTM International. (2025). ASTM D6304-25, Standard test method for determination of water in petroleum products, lubricating oils, and additives by coulometric Karl Fischer titration. https://store.astm.org/d6304-25.html
  4. Costello, M. J. (1993). Shaft voltages and rotating machinery. IEEE Transactions on Industry Applications, 29(2), 419–426. https://doi.org/10.1109/28.216553
  5. Graf, S., Koch, O., & Sauer, B. (2023). Influence of parasitic electric currents on an exemplary mineral-oil-based lubricant and the raceway surfaces of thrust bearings. Lubricants, 11(8), 313. https://doi.org/10.3390/lubricants11080313
  6. He, F., Xie, G., & Luo, J. (2020). Electrical bearing failures in electric vehicles. Friction, 8(1), 4–28. https://doi.org/10.1007/s40544-019-0356-5
  7. International Organization for Standardization [ISO]. (2017). ISO 15243:2017, Rolling bearings: Damage and failures: Terms, characteristics and causes. https://www.iso.org/standard/59619.html
  8. Iwase, S., Maruyama, T., Momozono, S., Maegawa, S., & Itoigawa, F. (2024). Studies on dielectric spectroscopy of oxidatively degraded poly(α-olefin). Frontiers in Mechanical Engineering, 10, 1504347. https://doi.org/10.3389/fmech.2024.1504347
  9. Mailula, K. O., & Saha, A. K. (2025). A comprehensive review of shaft voltages and bearing currents, measurements and monitoring systems in large turbogenerators. Energies, 18(8), 2067. https://doi.org/10.3390/en18082067
  10. Nippes, P. I. (2004). Early warning of developing problems in rotating machinery as provided by monitoring shaft voltages and grounding currents. IEEE Transactions on Energy Conversion, 19(2), 340–345.
  11. Puchtler, S., Maier, R., Kuhn, M., & Burkhardt, Y. (2024). The influence of load and speed on the initial breakdown of rolling bearings exposed to electrical currents. Lubricants, 12(1), 1. https://doi.org/10.3390/lubricants12010001
  12. Safdarzadeh, O., Farahi, A., Binder, A., Sezen, H., & Hofmann, J. P. (2024). WLI, XPS and SEM/FIB/EDS surface characterization of an electrically fluted bearing raceway. Lubricants, 12(5), 148. https://doi.org/10.3390/lubricants12050148
  13. Schneider, V., Behrendt, C., Höltje, P., Cornel, D., Becker-Dombrowsky, F. M., Puchtler, S., Gutiérrez Guzmán, F., Ponick, B., Jacobs, G., & Kirchner, E. (2022). Electrical bearing damage, a problem in the nano- and macro-range. Lubricants, 10(8), 194. https://doi.org/10.3390/lubricants10080194
  14. Zhou, F., Yang, K., & Wang, L. (2024). The effect of water content on engine oil monitoring based on physical and chemical indicators. Sensors, 24(4), 1289. https://doi.org/10.3390/s24041289

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.