KALTECKOREA

BlogApplication notes

Why do bearings show evenly spaced marks after shipping or standing idle?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Greases

Taking evenly spaced marks on a raceway for dents from a knock in transit and simply replacing the bearing is the usual response, but the marks may not be dents at all; they can be wear left where small movements at standstill pushed the lubricant film away, and they return if the conditions stay the same. What actually lies behind them can be vibration at standstill, oil that returns slowly to the contact, an unsuited thickener or grade, too little grease, missed shipping locks and periodic turning, or vibration from neighbouring machines, and sometimes two or more at once.

Background

A newly delivered machine is started for the first time, or duty is switched to a standby pump that has sat idle for months, and it hums and vibrates from the moment it turns. With the bearing out, the raceway shows a row of polished marks spaced exactly as far apart as the balls or rollers, some of them stained brown. The bearing has barely been used.

The loss does not end with the price of a bearing. For new equipment, commissioning slips and time goes into working out whether the damage came from shipping or installation; for a standby unit, it cannot be used just when it is needed. Such marks shorten bearing fatigue life, raise friction torque through wear, and are poorly predicted by standard life calculations (de la Presilla et al., 2023). Because damage done at rest shows only after running begins, its cause is also easy to miss.

This damage is called false brinelling. When the rolling elements and raceways of a stationary bearing move back and forth over a very small distance, fretting wear forms at the contacts, leaving deep craters with relatively polished bottoms, evenly spaced around the rings (Januszewski et al., 2023). It looks like true brinelling, where overload deforms the raceway plastically, but it forms in an entirely different way. Tiny movements under high contact pressure push the lubricant out of the contact, so metal touches metal and wears, and the particles and reaction products that break away have no way out and act as an abrasive that enlarges the damage (Grebe, 2013).

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: keep the marked bearing and the grease in it, measure whether the mark spacing matches the rolling element spacing, and record when, where and how the machine stood idle, together with the TDS of the grease it was filled with.

Hypothesis 1: rocking at standstill

Every situation in which a bearing stands still under load while vibration keeps passing through it belongs to this hypothesis. It often occurs when a lubricated bearing is stationary during transport by sea or rail, and it can occur in bearings that move through only a small part of their rotation in service (Sosa, 2023). Say an assembled gearbox was shipped over several days by truck and ship. At the first test run on site it makes a noise at a regular interval, and when it is opened the marks lie in a row along the lower part of the raceway.

How severe the damage gets depends on the ratio of the rolling element's travel to the contact width. In ball-on-flat experiments that reproduced the vibration, damage began at small asperity contacts and spread quickly over the whole contact with continued rubbing; it was worst when the travel was shorter than the contact width and dropped sharply once the travel exceeded it (Januszewski et al., 2023). In the same experiments, lower frequency and lower contact pressure gave less damage, and the contact ran in boundary lubrication at best, at times approaching dry conditions. With such short travel the contact is never fully exposed, so fresh lubricant can hardly get in, and under critical conditions the contact can be badly damaged within minutes, only a few thousand load cycles (Grebe, 2013).

Check first whether the mark spacing equals the rolling element spacing and whether the marks cluster on the loaded side. For shipping, find the route, the modes of transport and the days in transit; for idle periods, find how long the machine stood and what was running around it. For equipment that will face the same conditions again, an accelerometer on the housing of the stationary bearing shows how much it actually shakes in transit or while neighbouring machines run.

Once vibration at standstill is confirmed, the remedy depends on where it comes from. In transit, lock and support the shaft to cut the motion and load on the bearings; from neighbouring machines, break the path the vibration travels. Since lower contact pressure gave less damage in experiments (Januszewski et al., 2023), supports that take load off the bearings in transit or storage can also help. Where the vibration cannot be removed entirely, choose a grease suited to those conditions as well.

Hypothesis 2: slow oil return

This covers equipment shipped or left standing while filled with a high base oil viscosity grease meant for heavy loads, or a grease that gives up its oil reluctantly. Shipping in cold weather or storing in cold places makes the base oil thicker still, which adds weight to this hypothesis. A small gearbox filled with the grease used in heavy-duty gearboxes, arriving by sea in midwinter with raceway marks that the same gearbox shipped in summer did not have, is one such case.

How grease protects the contact depends on the oil its thickener releases. In oscillating contacts, refilling of the contact by bled oil through capillary forces has been identified as a key mechanism for preventing wear, and the onset of severe wear correlated strongly with the inlet length of the oil meniscus at the contact (Bayer et al., 2024). In bearing tests with lithium complex model greases too, the grease's ability to release plenty of highly mobile base oil into the rolling element's track was the crucial mechanism for preventing wear, especially at small oscillation angles (Wandel et al., 2022).

Base oil viscosity governs how fast that oil comes back. When the travel was shorter than the contact width, lower-viscosity oils and greases caused less damage (Januszewski et al., 2023), and another study comparing greases in a bearing test also found a clear link between base oil viscosity and the extent of damage, with temperature having a large effect on grease properties (Tetora et al., 2023). Lower viscosity is not better under every condition, though. In thrust ball bearing tests, grease with low-viscosity base oil reduced fretting wear better at high oscillation speed, and grease with high-viscosity base oil did so at low speed (Maruyama et al., 2017).

Find in the TDS the base oil viscosity and the oil separation result, which shows how readily the grease gives up its oil. Look at temperature records for shipping or storage too, if any exist. If marks cluster in winter shipments, and the same equipment filled with lower-viscosity grease shows fewer, this hypothesis gains weight.

For equipment that cannot avoid vibration in transit or on standby, review with the supplier a grease with low base oil viscosity that gives up its oil readily. In tests simulating rail and sea transport, among greases without the anti-wear additive ZDDP, damage fell by 97% with a grease whose less viscous oil bled abundantly from an open-structured thickener (Lin et al., 2022). Still, confirm against the bearing maker's recommended viscosity that such a grease also builds enough film under operating load and temperature.

Hypothesis 3: thickener and grade

Even with the same base oil, results differ with how stiff the grease is and what thickener it is made with. Look at this hypothesis for equipment given a stiff grease chosen with only rotation in service in mind, or where the factory-fill grease was set without regard to thickener type. Suppose that, of two models shipped from the same plant by the same route, only one keeps showing marks. It turns out the two were being shipped with different greases.

Consistency and thickener together set how firmly oil is held and how the grease flows. In vibration experiments, oils with their better flow generally prevented damage from lubricant shortage more effectively than greases, and among greases those with low base oil viscosity and a low NLGI grade had the advantage, though not uniformly (Grebe, 2013). Lithium and urea greases also caused somewhat more damage than oils with the same base oil (Januszewski et al., 2023). Yet the thickener can be useful in itself. In thrust ball bearing tests the thickener formed a layer that prevented fretting wear, and greases with polyurea or calcium sulfonate thickeners were effective in laboratory tests (Maruyama et al., 2017; Sosa, 2023).

List the greases of marked and unmarked equipment side by side, down to the NLGI grade and thickener type in each TDS. If the TDS gives a fretting test result, see how it was measured. The standard test for fretting wear protection by greases measures raceway wear in oscillating thrust ball bearings and ranks greases from low to high wear (ASTM International, 2024). Its oscillation angle of ±6°, however, is far larger than the ±0.5° of a test built to imitate standstill vibration, and with tests this different, good results in one do not mean good results in another that looks similar (Grebe & Widmann, 2023).

If thickener and grade look unsuited, ask suppliers for greases with test data under standstill vibration and compare them. If a stiff grease was in use, consider one grade softer; if the thickener holds its oil tightly, consider a thickener structure that releases oil readily. Confirm with the bearing maker that the new grease also suits the operating temperature and speed.

Hypothesis 4: too little grease

Suspect the grease quantity where bearings are packed by hand during assembly, where maintenance has no set fill quantity, or where parts ship with only rust-preventive oil and no grease. The same applies when, over a long idle period, grease has shifted to one side or dried out. The scene goes like this. Of several units of one model sent out on the same truck on the same day, only a few show marks, and opening their bearings reveals unusually little grease left beside the raceway.

At small amplitudes, the oil that wets the contact comes mainly from the bands of grease pushed aside along both edges of the rolling track (Liu et al., 2026). If the grease cannot send enough oil to the contact inlet, wear in the form of false brinelling and early failure can follow (Wandel et al., 2022). So when little grease is left beside the track, or what is left has dried, the reservoir that supplies the oil shrinks. Tests simulating sea and rail transport, in which a grease that bled oil abundantly cut damage sharply, fit the same picture: oil supply to the contact matters (Lin et al., 2022).

On opening a marked bearing, see how much grease is left beside the rolling elements and raceway, and whether any spots are dry or the grease has gathered to one side. Check the fill method and records in assembly and, if possible, weigh bearings before and after filling to find the actual quantity. If marked and unmarked units shared the same grease and route and differed only in fill quantity, this hypothesis is strong.

The first remedy is to take the fill out of guesswork. Control it with a metered dispenser or by weight, set to the bearing maker's recommended fill. Rather than packing in as much as possible, keep within the recommended range. For equipment that will stand for a long time, check the grease before shipping or storage, and refill bearings that have dried out.

Hypothesis 5: no lock, no turning

This covers cases where the shaft locks meant for shipping were never fitted or were left off, and cases where, with installation delayed, nobody turned the shaft during months in storage. Picture a site where construction is late and a fan delivered months ago still stands in its crate in a warehouse. The shaft lock for shipping was not in the crate, and the storage log shows no day on which the shaft was turned.

Damage in transit is an old problem. In the 1930s, periodic marks were found in the wheel bearing raceways of new cars delivered by ship or train, traced to the cars being rocked by the vibration of large ship diesel engines or by the jolt each time a wheel passed a rail joint (Grebe, 2013). Locking the shaft prevents the tiny back-and-forth movement of the rolling elements at one spot, and making sure the rolling elements do not rock in one position for long periods also helps (Sosa, 2023). A large turn moves the contact to a new spot. In experiments, once the amplitude was large enough, grease flowing between the rings became the main mechanism and reduced wear effectively (Liu et al., 2026).

Check the shipping specification and packing photos for a shaft lock, and whether a lock removed at installation is still around. Find the storage period, location and any record of periodic turning, and see whether the equipment maker's storage instructions give a turning interval. If marks appear only on units stored for a long time and not on those commissioned straight after delivery, look at storage; if they cluster on units shipped long distances, look at transport.

Procedure is what closes the gap left by missing locks and turning. Write shaft locking and support into the shipping specification, and record in the installation log when and by whom the locks were removed. In storage, turn the shaft by hand at the interval in the equipment maker's instructions so the rolling elements come to rest at a different spot each time, and log the date. For equipment facing long storage, review the grease choice before shipping as well.

Hypothesis 6: neighbouring machines

Where a standby unit sits right beside a running one, as with pumps, fans or generators installed in pairs with only one in service, suspect vibration from the neighbour. A shared baseplate, a common foundation or connecting pipework gives vibration a path across. Take a plant room where one of two cooling water pumps has stood in reserve for months. When duty is switched to it for maintenance, it is noisy from the first turn, while the bearings of the pump that was running are fine.

A standby unit is off most of the time and brought into service when needed, yet vibration from the running unit can damage the bearings of the one that is switched off. Such a unit may be noisy as soon as it starts and fail completely within days or weeks, even though everything else about it is new (Grebe, 2013). Vibration arriving from next door may look small, but small is no comfort: travel shorter than the contact width was exactly the condition that did the most damage (Januszewski et al., 2023).

Measure vibration at the bearing housings of the stationary standby unit while the running unit operates, and compare with the running unit stopped. Check on drawings and on site which of baseplate, foundation and pipework the two units share. If marks appear only on the standby unit, this hypothesis is strong.

If vibration from next door is the cause, separating paired units or isolating them mechanically is the way put forward to prevent the damage (Sosa, 2023). Review with the equipment maker splitting the shared baseplate or fitting anti-vibration mounts and flexible joints, and alternate duty between the two units on a set schedule so neither stands still for long. If the running unit itself vibrates heavily, fix that cause too.

Finding the cause

The six hypotheses fall into two groups: where the vibration that rocked the bearing came from, and how well the grease protected the contact under that vibration. The vibration side can be ruled out first from records. Transport route and locking, storage period and turning records, and the machines running nearby can all be checked before any bearing is opened.

Next comes the spread of the marks. Marks only on units that went through transport point first to transport locking, marks only on units stored for long periods to missed turning, and marks only on standby units to vibration from neighbouring machines. If only a few units on the same route and grease are marked, suspect fill quantity; if marks recur across all equipment on one grease and worsen in winter, look at the grease itself: base oil viscosity and bleed, and thickener.

If that does not settle it, run a control trial. Of two units going by the same route, lock the shaft on one only, or fill one only with the candidate grease, and inspect the bearings the same way on arrival. For a standby unit, compare vibration during periods with the running unit stopped and running. When choosing grease by laboratory test, pick a test that matches the vibration amplitude on site, because standard tests with different oscillation angles cannot stand in for each other (Grebe & Widmann, 2023).

Final confirmation comes with the next shipment or the next switch to standby. Inspect the bearings of equipment sent under the changed conditions on the same basis, and log whether the marks have gone and whether noise and vibration at commissioning are normal. Recording damage in the terms and characteristics of the bearing damage classification standard makes comparison easier when the same symptom returns (ISO, 2017).

The hypotheses can overlap. Vibration causes the damage and grease slows it, so both can hold at once. In that case, reduce the vibration first. Of six industrial greases tested under wind turbine pitch bearing conditions, none reduced wear under every condition (Schwack et al., 2020), and model greases did not prevent false brinelling completely but only slowed its progress (Grebe, 2013). Treat a grease change as the step that lowers the risk remaining after the vibration has been reduced.

Limits and cautions

Suitable vibration limits, grease fill and turning intervals in storage differ by bearing and equipment, so numeric decisions follow the bearing and equipment makers' instructions and the grease's TDS. Whether a mark is true brinelling, false brinelling or another form of damage such as electrical erosion can be hard to tell by appearance alone, so get confirmation from the bearing maker or a damage analysis specialist. False brinelling marks are not merely cosmetic but signal early damage that progresses rapidly from the first cracks and particles, so lean towards not reusing a marked bearing (Grebe, 2013).

Safety matters too. Turn shafts by hand or dismantle bearings only with the equipment fully stopped and locked out, and block automatic start on standby units. After removing shipping locks, check that none remain before running. For greases and cleaning agents, wear protective equipment as the product's safety data sheet, the SDS, directs.

Sources

  1. ASTM International. (2024). ASTM D4170-24, Standard test method for fretting wear protection by lubricating greases. https://store.astm.org/d4170-24.html
  2. Bayer, G., Wandel, S., Ayromlou, A., Bader, N., & Poll, G. (2024). Influence of the meniscus on wear in grease-lubricated oscillating rolling contacts. Tribology International, 197, 109771. https://doi.org/10.1016/j.triboint.2024.109771
  3. de la Presilla, R., Wandel, S., Stammler, M., Grebe, M., Poll, G., & Glavatskih, S. B. (2023). Oscillating rolling element bearings: A review of tribotesting and analysis approaches. Tribology International, 188, 108805. https://doi.org/10.1016/j.triboint.2023.108805
  4. Grebe, M. (2013). New investigations and approaches to explain standstill marks on roller bearings (false brinelling). Faculty of Materials Science and Technology in Trnava, Slovak University of Technology. https://www.mtf.stuba.sk/buxus/docs/internetovy_casopis/2013/1/1_Grebe.pdf
  5. Grebe, M., & Widmann, A. (2023). Comparison of different standard test methods for evaluating greases for rolling bearings under vibration load or at small oscillation angles. Lubricants, 11(7), 311. https://doi.org/10.3390/lubricants11070311
  6. International Organization for Standardization [ISO]. (2017). ISO 15243:2017, Rolling bearings – Damage and failures – Terms, characteristics and causes. https://www.iso.org/standard/59619.html
  7. Januszewski, R., Brizmer, V., & Kadiric, A. (2023). Effect of lubricant properties and contact conditions on false brinelling damage. Tribology Transactions, 66(2), 350–363. https://doi.org/10.1080/10402004.2023.2183915
  8. Lin, C.-L., Fallahnezhad, K., Brinji, O., & Meehan, P. A. (2022). Mitigation of false brinelling in a roller bearing: A case study of four types of greases. Tribology Letters, 70(1), 22. https://doi.org/10.1007/s11249-021-01557-0
  9. Liu, M., Wandel, S., Bader, N., Lin, Z., Bayer, G., Poll, G., & Marian, M. (2026). Beyond starvation: Amplitude-dependent grease replenishment mechanisms in oscillating rolling bearings. Tribology International, 214, 111354. https://doi.org/10.1016/j.triboint.2025.111354
  10. Maruyama, T., Saitoh, T., & Yokouchi, A. (2017). Differences in mechanisms for fretting wear reduction between oil and grease lubrication. Tribology Transactions, 60(3), 497–505. https://doi.org/10.1080/10402004.2016.1180469
  11. Schwack, F., Bader, N., Leckner, J., Demaille, C., & Poll, G. (2020). A study of grease lubricants under wind turbine pitch bearing conditions. Wear, 454–455, 203335. https://doi.org/10.1016/j.wear.2020.203335
  12. Sosa, Y. (2023, June). False brinelling: An increasing type of a rolling bearing wear. Tribology & Lubrication Technology. Society of Tribologists and Lubrication Engineers. https://www.stle.org/files/TLTArchives/2023/06_June/Feature.aspx
  13. Tetora, S., Schadow, C., & Bartel, D. (2023). Influence of grease properties on false brinelling damage of rolling bearings. Lubricants, 11(7), 279. https://doi.org/10.3390/lubricants11070279
  14. Wandel, S., Bader, N., Glodowski, J., Lehnhardt, B., Leckner, J., Schwack, F., & Poll, G. (2022). Starvation and re-lubrication in oscillating bearings: Influence of grease parameters. Tribology Letters, 70(4), 114. https://doi.org/10.1007/s11249-022-01655-7

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.