KALTECKOREA

BlogApplication notes

Why does grinding leave burn marks and cracks?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Cutting the feed or the depth of cut is the usual response to grinding burn, but that only trades away output to make less heat, and whatever stopped the heat from being carried away is still there. What actually lies behind it can be grinding fluid held off by the air layer round the wheel, too little flow or a misplaced nozzle, weak lubrication, fines in the fluid, a dull or loaded wheel or hot fluid, and sometimes two or more at once.

Background

Gear flanks, bearing raceways and camshafts that have already been heat treated come off the grinder with brown or bluish bands on the surface. This grinding burn shows up dark in an acid etch inspection, and on bad parts magnetic particle inspection can reveal fine cracks in a network. Grinding is usually the last operation, so a part scrapped here carries the cost of all the machining and heat treatment before it. The bigger problem is burn that cannot be seen: a part that looks sound can be shipped and fail by fatigue in service.

Most of the energy put into grinding turns into heat. In shallow-cut grinding with conventional wheels, about 60 to 85% of that heat has been estimated to enter the workpiece (Malkin & Guo, 2007). Burn appears when this heat raises the surface far enough to show discolouration and blemishes, but it can occur with no visible flaw at all. As surface temperature rises, the microstructure changes and the hardness with it, and tensile residual stress left at the surface shortens fatigue life (Irani et al., 2005). Burn can therefore show as a drop in surface hardness or as rehardening, where the surface is quenched hard again (Gurruchaga et al., 2023).

Grinding cracks are the same heat taken one step further. In carburised and hardened steel parts, grinding cracks have been reported to form when overheating of the surface leaves tensile residual stress above the fracture strength of the steel, with an apparent link to the amount of retained austenite (Buenneke, 1972). Grinding fluid reduces friction so less heat forms, carries away the heat that does form, and flushes out chips (Brinksmeier et al., 1999). The causes therefore split into those that make more heat and those that keep the heat from getting away.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: keep the burnt parts aside, note where on the part the marks are and how many parts after the last dressing they appeared, with the wheel speed and the fluid's flow, concentration and temperature at the time, and compare them with the grinding fluid's technical data sheet, the TDS, and the grinding parameter sheet.

Hypothesis 1: wheel air barrier

If burn began after the wheel speed was raised to cut cycle time, suspect the air layer first. It tends to arise with large-diameter wheels, on machines that pour fluid through wide low-pressure nozzles, and where the nozzle aims at the workpiece rather than the contact zone. Stand in front of such a grinder after the speed increase: fluid gushes from the nozzle but fans out and splashes before it reaches the wheel, while sparks and steam rise where wheel and workpiece meet.

A fast-turning wheel drags a layer of air round with it (Ebbrell et al., 2000). When this air layer pushes aside a slow jet of fluid, the share of the nozzle's output that actually passes between wheel and workpiece shrinks. In tests that used very high jet velocities to break through the air barrier, the faster the jet the better the grinding results, and shoe nozzles, which sit against the wheel face and carry fluid along at wheel speed, prevented a vapour film forming in the contact zone and pushed thermal damage out to higher removal rates (Irani et al., 2005). Matching the jet velocity closely to the wheel's peripheral speed is recommended (Morgan et al., 2008).

Look first. With the machine running, see whether the fluid jet clings to the wheel and is drawn into the contact zone or bounces off in front of it. Then do the numbers. Dividing the flow leaving the nozzle by the nozzle outlet area gives a rough jet velocity; compare it with the peripheral speed worked out from wheel diameter and spindle speed. If the jet is far slower than the wheel and the burn coincides with the speed increase, this hypothesis gains weight.

If the air layer looks responsible, change the nozzle so the fluid breaks through it. Narrow the nozzle outlet or raise the pressure to bring jet velocity up towards the wheel's peripheral speed, and aim a nozzle that gives a coherent, non-spreading jet squarely at the contact zone. Fitting a plate ahead of the nozzle to scrape off the air layer, or reviewing a shoe nozzle that sits against the wheel with the machine builder, are other options. Even after these changes, check whether the grinding parameters need resetting for the higher speed.

Hypothesis 2: flow and nozzle setup

Nozzles lose their place more easily than expected. They get knocked off line during a wheel change or a setup, and as the wheel wears smaller the gap between nozzle tip and contact zone grows. Nozzle holes block with swarf, pressure drops as the pump wears and filters clog, and on a central supply line flow falls when other machines run at the same time. One example is a grinder that was fine in the week a new wheel went on, but shows a darker brown band at the same spot on the ground face as the wheel gets smaller.

Not all the fluid leaving a nozzle passes through the contact zone. A study that moved the nozzle between three positions and measured the flow through the contact zone found that the amount differed with position (Ebbrell et al., 2000). There are also results showing more flow through the contact zone with the nozzle closer to it. When too little fluid reaches the contact zone, the nature of the cooling changes. At first small bubbles boil off the work surface and draw heat away well, but as temperature rises further the boiling turns to film boiling, where a vapour film lies between workpiece and fluid; that film blocks heat transfer, the surface temperature climbs quickly and the surface burns. For water-based fluids this film boiling temperature has been reported as 100 to 120°C (Irani et al., 2005).

Flow is known once it is caught. Hold a container at the nozzle tip, measure what collects in a set time, and compare it with the flow in the parameter sheet or machine specification, along with the pump outlet pressure gauge and the pressure difference across the filter. Photograph the distance and aim between nozzle tip and contact zone just after a wheel change and again once the wheel has worn down, and compare. Burn that gathers late in the wheel's life, or at times when other machines are running too, is grounds to suspect the supply side.

If supply looks short, make flow and nozzle position managed items. Give the nozzle an adjustment range and reference marks so it can follow the contact zone as the wheel wears, and check its aim at every wheel change. Clean nozzles and filters at fixed intervals and log the caught flow regularly. On a central system, check with the facilities staff that supply pressure at the grinder does not swing when other machines start.

Hypothesis 3: weak lubrication

If burn increased after a switch from oil-based to water-miscible grinding fluid for cost or fire-safety reasons, or from one water-miscible fluid to a synthetic type with fewer lubricating ingredients, lubrication may have weakened. The same applies to a sump whose concentration has fallen below the TDS range because evaporation was made up with water alone, and to jobs that moved to harder or tougher steels. Same wheel, same parameters, yet from the day after the fluid change the grinding sound turns sharper and the spindle load meter reads higher than before.

Grinding fluid does not only cool; by reducing friction between abrasive grains and workpiece it cuts the amount of heat formed in the first place (Brinksmeier et al., 1999). Raising the concentration of oil in a water-miscible grinding fluid has been reported to lower grinding forces, grinding energy and temperature while extending wheel life. By type, straight oils offer the best lubricity, while synthetics lead in heat removal and ease of filtering (Irani et al., 2005). When lubrication weakens, removing the same stock takes more energy, and most of it becomes heat that enters the workpiece.

Measure concentration with a refractometer, apply the supplier's correction factor and compare with the TDS range. Refractometer readings can be thrown off by tramp oil and contamination, so if the supplier specifies another method, use it as well (Byers, 2017). If spindle load or power can be logged, compare before and after the fluid change, and before and after the concentration is corrected, on the same part under the same parameters. Check the application section of the TDS too, to see whether the fluid in use is made for that steel and that kind of grinding.

If concentration was low, bring it back into the TDS range and top up with premix at the set concentration rather than water alone. If the change of fluid type looks responsible, run alternating trials of the old and new fluids on the same part together with the supplier to decide whether a grinding product with stronger lubrication is needed. Meanwhile, lower the depth of cut or feed to prevent burn, and raise them again once the cause is found.

Hypothesis 4: fines in the fluid

Grinding swarf is very fine, and it carries abrasive grains shed from the wheel as well. This hypothesis gains strength on machines whose filtration cannot keep up with these fines, where filter paper or cartridges are changed late, and in sumps whose settling tank is full of sludge. In a sump with only a magnetic separator, the non-magnetic abrasive grains keep circulating. Push a rod into the bottom of the sump and it comes out thick with grey sludge, and the ground face shows fine scratches and wave-like marks alongside the burn.

Fines that escape filtration go back between wheel and workpiece. In tests grinding steel with corundum particles added to the fluid, surface waviness rose markedly; this was put down to the particles blocking the wheel's pores and being carried into the grinding gap, wearing the wheel abnormally and making the actual depth of cut vary from spot to spot (Beekhuis, 2013). If chips are not flushed away the wheel clogs as if dull, and grains only plough and rub instead of cutting, so grinding forces, energy and the heat entering the workpiece rise sharply (Irani et al., 2005). Fines that block nozzle holes also cut the flow, as in the previous hypothesis.

Catch fluid from the nozzle in a clear bottle and let it stand a while; the fines that settle can be compared with new fluid. For a firmer figure, filter a set volume through filter paper, dry and weigh it, and compare readings taken just after and just before a filter change. Look up the type of filtration, the particle size it can remove, the filter change interval and the dates the settling tank was cleaned, and see whether burn and scratches gather towards the end of the filter change interval.

If filtration is not keeping up with the fines, match it to the grinding swarf. Add filter paper or centrifugal separation to the magnetic separator so non-magnetic abrasive grains are removed too, and change filters by pressure difference or at set intervals. Remove sludge from the settling tank and sump bottom regularly, and if a lot has built up, empty and clean the sump before refilling with new fluid. Check with the equipment supplier that filter capacity suits the number of grinders and the amount of swarf.

Hypothesis 5: dull or loaded wheel

If the first few parts after dressing are clean but burn deepens as the next dressing approaches, look at the wheel face. It happens when the dressing interval has been stretched to raise output, when dressing was too fine, when soft, gummy work material sticks to the wheel, and when the wheel is too hard for the material. Stop the wheel near the end of a cycle and shine a light across it at an angle: a band of shiny glaze shows, and in places metal is embedded and the wheel face looks dark.

Abrasive grains wear in use, and flats form at their tips. These flats cannot cut the workpiece, only rub it, so as their area grows grinding forces and power rise, and the heat needed to remove the same stock increases until it ends in burn. A wheel whose pores are packed with swarf gives the same result as one with more rubbing area. Dressing breaks dull grains and opens clogged pores to restore a sharp face, and the dressing conditions change how sharp the wheel face is and how much grinding power it draws (Malkin & Guo, 2008).

Setting the dressing log beside the burn log is the first check. Count how many parts after dressing the burnt ones appear, and if spindle power can be logged, see how it climbs within a dressing cycle. Examine the wheel face under a raking light for glazing and embedded metal, and check dressing depth, dressing feed and the condition of the dresser against the parameter sheet. Confirm from the wheel maker's data that the wheel specification suits the material.

If the wheel is the cause, rework the dressing. Set the dressing interval not by part count alone but so the wheel is dressed once power has risen by a set amount, and follow the wheel maker's recommended dressing depth and feed so the face is not closed up too fine. Replace a worn dresser. If the material tends to load the wheel, choose the wheel grade and structure again with the wheel maker, and consider fitting a cleaning nozzle that washes the wheel face.

Hypothesis 6: hot grinding fluid

Grinding fluid temperature rises easily in summer, on grinders with small sumps, in heavy roughing with high removal, and when the chiller is off or too small. On a central system with a distant tank, the fluid can also warm up in the pipework. Think of a plant where parts from the morning shift are clean but parts from the afternoon shift come out burnt. In the afternoon a hand in the sump finds the fluid more than lukewarm, and the chiller's indicator light is off.

The grinding fluid's power to remove heat comes from the temperature difference between workpiece and fluid, so the colder the fluid, the better it carries heat away (Irani et al., 2005). How much cooling matters shows clearly in creep-feed grinding with deep cuts. There, the share of heat entering the workpiece was as low as about 5%, which was attributed to cooling by the grinding fluid (Malkin & Guo, 2007). Warmed fluid enters the contact zone already hot, so for the same heat input it approaches the film boiling temperature described earlier sooner.

Temperature only shows when it is measured several times a day. Measure and log the fluid temperature in the sump and at the nozzle outlet every shift, and set it against the times burnt parts appeared. If there is a chiller, check its set point, the temperature difference across it, and any clogging of its filter and heat exchanger. See as well whether concentration shifts as water evaporates faster in the heat.

If hot fluid proves to be the cause, restore the cooling first. Service the chiller or increase its capacity, and if the sump is small, work with the equipment supplier on ways to give the fluid longer in the tank. Keep fluid temperature within the range the supplier and machine builder recommend, and rescheduling so heavy-removal jobs do not pile up in the hottest hours also helps.

Finding the cause

There is no need to search all six hypotheses at once. Rule them out starting with what is easiest to check. Concentration, fluid temperature, caught flow and the distance and aim of the nozzle take minutes, and the dressing and filter change records already exist. Changing the jet velocity or the wheel specification takes time and money, so it comes after.

When the burn appears is a strong clue. Burn that has persisted since the wheel speed went up points to the air layer and the nozzle; burn that grows as the wheel gets smaller points to nozzle distance and flow. Burn that deepens towards the end of the dressing cycle points to a dull or loaded wheel, burn concentrated in afternoons or summer to fluid temperature, and burn since a fluid change or water-only top-ups to lubrication and concentration. Burn accompanied by fine scratches and wave marks that follows the filter change cycle points to fines in the fluid.

If that does not settle it, run control trials. On the same part under the same parameters, change one thing at a time: grind straight after dressing, realign the nozzle to the contact zone, grind with fresh fluid made up at TDS concentration or with cooled fluid. After each change, check for burn with the same inspection method and count burnt parts per set quantity on the same basis as before.

The verdict comes from inspection. There is a standard method for detecting and classifying localised overheating on ground steel parts by chemical etching, which is not used on nitrided parts or stainless steels (ISO, 2017). To inspect without damaging the part, use Barkhausen noise measurement; the signal is sensitive to the hardness and residual stress of steel and is used to detect burn and judge its severity (Gurruchaga et al., 2023). Look for cracks in suspect parts with magnetic particle inspection, and measure surface residual stress by X-ray diffraction to narrow the cause (Buenneke, 1972).

The hypotheses often overlap. Fines clog both wheel and nozzle, a dull wheel makes more heat, the air layer and short flow carry less of it away, and hot fluid eats into whatever margin remains. In such cases first put right what gets fluid to the contact zone, meaning flow, nozzle and jet velocity, along with concentration and temperature, then dressing and the wheel, and last the grinding parameters, because while the fluid supply is unsettled, the effect of changing the wheel or the parameters cannot be compared fairly.

Limits and cautions

Suitable wheel peripheral speed, dressing conditions, fluid concentration and temperature, and flow differ by wheel, machine, material and fluid, so numeric decisions follow each maker's guidance and the grinding fluid's TDS. Judging burn and cracks, and whether burnt parts can be reground and used, is work for the quality engineer and the laboratory, and parts where fatigue matters, such as gears and bearings, are not released on a visual check alone. A wheel must never run above its rated maximum speed, so before changing speed confirm the limits from the wheel and machine makers.

Safety matters too. For the acids and solvents used in etch inspection, follow the product's safety data sheet, the SDS, for protective equipment and ventilation. Metalworking fluids can harm health through skin contact and through breathing in mist (OSHA, n.d.), and the US National Institute for Occupational Safety and Health has set out a recommended exposure limit and control methods for reducing exposure to them (NIOSH, 1998). Adjust nozzles or inspect the wheel face only after the machine is fully stopped and locked out, and never run a wheel with its guard removed.

Sources

  1. Beekhuis, B. (2013). Influence of solid contaminants in metal working fluids on the grinding process. Advanced Materials Research, 769, 61–68. https://doi.org/10.4028/www.scientific.net/AMR.769.61
  2. Brinksmeier, E., Heinzel, C., & Wittmann, M. (1999). Friction, cooling and lubrication in grinding. CIRP Annals, 48(2), 581–598. https://doi.org/10.1016/S0007-8506(07)63236-3
  3. Buenneke, R. W. (1972). Applications of residual stress measurements (SAE Technical Paper 720243). SAE International. https://doi.org/10.4271/720243
  4. Byers, J. P. (Ed.). (2017). Metalworking fluids (3rd ed.). CRC Press.
  5. Ebbrell, S., Woolley, N. H., Tridimas, Y. D., Allanson, D. R., & Rowe, W. B. (2000). The effects of cutting fluid application methods on the grinding process. International Journal of Machine Tools and Manufacture, 40(2), 209–223. https://doi.org/10.1016/S0890-6955(99)00060-7
  6. Gurruchaga, K., Lasaosa, A., Artetxe, I., & Martínez-de-Guerenu, A. (2023). Grinding burn detection via magnetic Barkhausen noise analysis independently of induction hardened depth. Materials, 16(5), 2127. https://doi.org/10.3390/ma16052127
  7. International Organization for Standardization [ISO]. (2017). ISO 14104:2017, Gears — Surface temper etch inspection after grinding, chemical method. https://www.iso.org/standard/70396.html
  8. Irani, R. A., Bauer, R. J., & Warkentin, A. (2005). A review of cutting fluid application in the grinding process. International Journal of Machine Tools and Manufacture, 45(15), 1696–1705. https://doi.org/10.1016/j.ijmachtools.2005.03.006
  9. Malkin, S., & Guo, C. (2007). Thermal analysis of grinding. CIRP Annals, 56(2), 760–782. https://doi.org/10.1016/j.cirp.2007.10.005
  10. Malkin, S., & Guo, C. (2008). Grinding technology: Theory and applications of machining with abrasives (2nd ed.). Industrial Press.
  11. Morgan, M. N., Jackson, A. R., Wu, H., Baines-Jones, V., Batako, A., & Rowe, W. B. (2008). Optimisation of fluid application in grinding. CIRP Annals, 57(1), 363–366. https://doi.org/10.1016/j.cirp.2008.03.090
  12. National Institute for Occupational Safety and Health [NIOSH]. (1998). Criteria for a recommended standard: Occupational exposure to metalworking fluids. DHHS (NIOSH) Publication No. 98-102. https://www.cdc.gov/niosh/docs/98-102/
  13. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.