Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Treating red carbide grinding fluid as fluid that is simply old and dirty, and changing the tank or just watching the colour, is the usual response, but the colour can be a sign that cobalt, the binder in the carbide, is dissolving into the fluid, so the same thing tends to come back in fresh fluid. What actually lies behind it can be amines and chelators that hold cobalt, pH out of range, carbide fines that stay in the fluid, a warm fluid or too little cobalt inhibitor, and sometimes two or more at once.

Background

In the tank of a grinder that resharpens carbide end mills and drills, a fluid that started out clear deepens over a few weeks through pink to the colour of red wine. Around the same time, word goes round that edges on freshly ground tools chip early, or that the edge surface looks crumbly under magnification. Tools need regrinding more often, tools with weak edges have shorter lives at the customer's site, and above all, cobalt dissolved in the fluid can be a problem for the lungs and skin of people working nearby.

Cemented carbide, often just called carbide, is a material in which very hard tungsten carbide grains are held together by metallic cobalt. In a water-mixed grinding fluid the two do not hold up equally. In corrosion studies the cobalt binder dissolved before the tungsten carbide, leaving tungsten carbide grains exposed where binder had gone, and the binder corroded most readily on the acidic side (Human & Exner, 1997). Divalent cobalt ions dissolved in water are pink, and cobalt forms complexes of various colours depending on what it is bound to (Greenwood & Earnshaw, 1997).

So the reddening colour and the weakening edge can be two faces of one process. When binder dissolves from the edge surface freshly exposed by grinding, the tungsten carbide grains there lose the metal that held them, and the dissolved cobalt builds up in the fluid and changes its colour. Fluid colour can also change because of dyes or tramp oil, so do not conclude from colour alone; confirm by measuring the cobalt concentration in the fluid.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: take a fluid sample, measure cobalt content, pH and concentration, gather the records of when the colour began to change and of tank changes, top-ups and workload, and compare them with the fluid's technical data sheet, the TDS.

Hypothesis 1: amines and chelators

This hypothesis comes up first in shops that use a general-purpose water-miscible fluid, chosen for cutting or grinding steel, unchanged on carbide, or that have chosen a fluid generously dosed with amines or chelators for rust protection and hard water. Amines are widely used in water-mixed fluids to hold alkalinity and prevent rust, and chelators are ingredients that hold metal ions in the water so they do not precipitate. Take a shop whose steel-part grinders and carbide-tool grinders share one type of fluid. The steel side tank keeps its colour for months, while only the carbide side tank turns red within weeks.

The route by which amines draw out cobalt is complex formation. In a study that soaked and rubbed carbide in triethanolamine solution and ran electrochemical tests, triethanolamine readily formed coordination compounds, complexes that surround and hold a metal ion, with cobalt ions, and the amount of cobalt dissolved rose with time and with triethanolamine concentration. The same study advises avoiding water-based cutting fluids containing triethanolamine with carbide tools (Zhang et al., 2010). If cobalt on the surface turned into ions but stayed put, dissolution would slow, but ingredients that form complexes carry the ions off into the fluid and let surface cobalt keep dissolving. That amine additives leach cobalt from carbide also came out of other tests on grinding fluid additives (Zhang et al., 2009).

Check the composition sections of the TDS and the safety data sheet, the SDS, for amines and chelators, and see whether the product states that it was designed with cobalt leaching in mind for carbide grinding. If the same fluid serves both steel and carbide, measure the colour and cobalt content of both tanks on the same day and set them side by side. When sending samples to a laboratory, record the cobalt result with the sampling date and the days since the tank was filled, so the rise over time can be seen.

Once the composition is the suspect, review with the supplier a change to a fluid made for carbide grinding with low cobalt leaching, and if steel and carbide share one fluid, give the carbide side its own tank. Before switching, soak carbide test pieces or carbide grinding sludge in the current and candidate fluids under the same conditions and compare cobalt content; this immersion test shows the difference in numbers before the fluid goes into service.

Hypothesis 2: pH out of range

pH drifts out of the TDS range when the fluid has gone lean, when microbes have grown in long-used fluid, or when topping up is done with water alone or another chemical has got in. On the other hand, repeated doses of alkaline booster to hold pH can push the amine content above the original design. Consider the day a grinder restarts after standing idle for two weeks over the holidays. The tank smells sour, the pH strip shows a lower colour than usual, and that week the fluid colour deepens unusually fast.

Corrosion of the cobalt binder depends strongly on pH. On the acidic side the binder corrodes and dissolves most readily (Human & Exner, 1997). In a study that corroded carbide in acidic, neutral and alkaline solutions and then measured the strength left, the corrosion rate was lower in alkaline solution, and the effect on strength in neutral and alkaline solutions was far smaller than in acid (Zheng et al., 2019). Holding pH high is not the whole answer, though. Triethanolamine solution is alkaline, yet it dissolved cobalt by forming complexes, so in a fluid whose high pH is held by amines, the complex route stays open (Zhang et al., 2010). Too low a pH lets acid attack the binder, and a pH held up by repeated amine additions lets complexes do it.

Measure pH with a calibrated pH meter rather than a strip, record it with concentration, and compare both with the TDS ranges. If pH is low, tell whether the fluid has gone lean or microbes have grown, using odour, dip slides for bacteria and the concentration reading. If cobalt keeps rising while pH is in range, find in the records the type and amount of alkaline booster added so far, and work out with the supplier how much amine may have built up.

Bring an out-of-range pH back by fixing its cause. If the fluid is lean, correct the concentration; if microbes have grown, clean the tank and refill; and avoid simply lifting the number with alkaline booster. When a booster is needed, confirm with the supplier that it is fit for carbide. When machines stand idle for long periods, keep the fluid circulating or set a rule to check pH and odour before restart.

Hypothesis 3: fines left in fluid

Grinding carbide produces very fine carbide powder. In small tanks that rely only on settling, machines with no filter or coarse filter media, tanks whose sludge is seldom removed, and shops that run fluid for a long time between changes, this powder circulates in the fluid or lies on the bottom, in contact with the fluid for a long time. The case looks like this: stirring the bottom of a tank whose sludge has not been removed for months lifts a thick black mud-like sludge, and its fluid is always a shade redder than that of the next machine, whose sludge is removed often.

The amount of cobalt that dissolves depends on how much cobalt surface is exposed to the fluid and for how long. Grinding fines have far more surface area than a lump of the same weight, and cobalt binder is exposed on every bit of that surface. In tests with triethanolamine solution, dissolved cobalt rose with immersion time, so the longer fines stay in the fluid, the more cobalt can build up in it (Zhang et al., 2010). In practice, a study of a carbide-tipped saw blade grinding shop found elevated cobalt in the grinding fluid, and a survey of fluids from nine carbide grinding shops indicated that such elevated levels may be common (Stebbins et al., 1992). A survey of Finnish workplaces also found a high mean cobalt concentration in grinding fluids and recommends changing the fluids more often (Linnainmaa et al., 1996).

Catch fluid in a bottle, let it stand overnight and see how much black powder settles to the bottom. Note the thickness of sludge on the tank bottom, whether there is a filter and the state of its media, the last day sludge was removed and the last day the fluid was changed. Comparing, by the same method, how fast cobalt content rises before and after removing the sludge shows how much the fines contribute to the rise in cobalt.

If the fines look to be one of the causes, the key is to get them out of the fluid quickly. Fit fine filtration to carbide grinders, remove sludge from settling tanks on a fixed schedule, and set the fluid change interval by cobalt content. Removed carbide sludge is waste that carries cobalt, so dispose of it under local rules and check whether a recycler will take it.

Hypothesis 4: warm fluid

Fluid temperature rises when several machines run nonstop from a small tank with no chiller, in poorly ventilated grinding rooms in summer, and on days of deep grinding with high power or of large tools. Sometimes the tank sits against the machine body or hydraulic unit and picks up its heat too. On a midsummer afternoon, warm air rises when the tank lid is lifted, and the tank wall feels warm to the hand. Around then, people remark that the fluid reddens noticeably faster than in winter.

Part of the heat from grinding passes into the fluid, which is exactly the cooling the fluid is there to do (Irani et al., 2005). If the heated fluid cannot cool enough in the tank, the temperature of the whole charge creeps up over the day. Chemical reactions generally speed up as temperature rises, so the reactions that dissolve binder and form complexes can also run faster in warm fluid (Atkins & de Paula, 2014). In the grinding zone the effect may be larger still. A freshly ground edge surface is momentarily hot and has just exposed new cobalt, and it meets the fluid right there.

Measure tank temperature a few times a day, just after start-up and at the busiest time of the afternoon, and compare it with the temperature recommended in the fluid's TDS or by the supplier. If there is a chiller, see from the temperature difference between fluid in and out whether it is doing its job; if not, ask whether the tank volume suits the number of machines and the workload. If there are cobalt records by season, lay them over the temperature records to see whether cobalt rose faster in hot weather.

High temperature calls first for ways to cool the fluid. Fit a chiller or increase tank volume, move the tank away from heat sources, and improve ventilation in the grinding room. For heat-heavy work such as deep grinding, keep fluid flow generous within the machine limits. After bringing the temperature down, measure the cobalt rise over the same period again to confirm the effect.

Hypothesis 5: too little inhibitor

If a fluid sold for carbide still turns red, check whether there is enough cobalt inhibitor. This happens when a fluid has been run for a long time with mostly water top-ups, when a booster other than the concentrate has been mixed in, or when old fluid was left in the tank during a product change. A carbide-grinding fluid that stayed clear for the first few months slowly starts to turn pink from some point on. Concentration and pH sit within the TDS ranges, yet the colour does not come back.

A cobalt inhibitor typically slows the dissolution of binder into the fluid by forming a film on the carbide surface or by changing cobalt into a form that stays bound. In tests with triethanolamine solution, adding triethanolamine oleate clearly reduced cobalt leaching, and adding it together with borax worked best (Zhang et al., 2006). In follow-up tests by the same group, benzotriazole, known as a copper corrosion inhibitor, also reduced cobalt leaching, and a mixture of triethanolamine oleate, borax and benzotriazole gave the best inhibition (Zhang et al., 2009). If inhibitor is used up on surfaces or carried off with grinding sludge, and top-ups are mostly water rather than concentrate, inhibitor content can fall below the design level.

First check in the TDS whether the product claims cobalt inhibition and over what concentration range the effect holds. Find the ratio of concentrate to water in the top-up records, and ask the supplier whether the inhibitor content of the used fluid can be analysed. The most direct check is an immersion test. Soak identical carbide test pieces in fresh fluid and in the fluid in use for the same time at the same temperature and compare how much cobalt content rises in each; that shows how much inhibition has been lost in service.

If inhibitor turns out short, restore it by adding concentrate or an inhibitor booster as the supplier specifies, and top up from now on with premixed fluid rather than water. If cobalt keeps rising after that, it is better to drain, clean and refill the tank, since cobalt and fines built up in old fluid do not go away with fresh inhibitor alone.

Finding the cause

There is no need to dig into all five hypotheses at once. pH, concentration and temperature take a few minutes on the floor, and sludge levels and top-up records are in the tank and the log. Checking the composition means reading the TDS and SDS, and cobalt content and immersion tests go to a laboratory, so send the samples together. Finishing the floor measurements and sampling on the first day lets other causes be ruled out while waiting for results.

The first clue is when, and in which tank, the colour changed. If even a fresh tank reddens within weeks, look first at the fluid composition, amines and chelators; if it stays clear for months and then reddens slowly, look first at lost inhibitor or built-up fines. If it speeds up only in summer, put temperature first, and if it follows a long stoppage or comes with odour, put pH first. If steel and carbide share a fluid and only the carbide side reddens, the problem lies in the pairing of carbide and fluid rather than in the fluid alone.

The way the edge has weakened is also a clue. On a surface where binder has dissolved, tungsten carbide grains are exposed without the metal that held them, so look under magnification for hollows between grains at the edge. Such corrosion pits on the binder side become places where stress concentrates and sharply reduce the strength of carbide (Tarragó et al., 2014). If edge chipping shows even straight after grinding, suspect grinding conditions or the wheel as well; if it is worse on tools that stayed in contact with fluid longer, lean towards the fluid.

If that still does not settle it, run control trials that change one thing at a time. Soak identical carbide test pieces for the same time in the current fluid, fresh fluid, fluid with pH corrected, fluid with fines filtered out and cooled fluid, and compare how much cobalt content rises in each; that shows at laboratory scale what changes leaching most. The approach of a study that combined immersion, friction and electrochemical tests to examine cobalt leaching is a useful reference (Zhang et al., 2010). On the floor, change one thing at a time and compare the cobalt rise over the same period and the condition of edges on the same basis as before the change.

The hypotheses can overlap. In an amine-rich fluid where fines linger and the weather is hot, all three drive leaching up at once, and in a fluid short of inhibitor even a small swing in pH changes the colour quickly. In such cases clean the tank and refill with a fluid suited to carbide, put filtration and temperature right, and hold pH and concentration within range. Measuring cobalt content at intervals under those conditions and watching how fast it rises reveals whether any cause remains.

Limits and cautions

Suitable pH, concentration, temperature and fluid change interval differ by fluid, carbide grade, machine and workload, so numeric decisions follow the fluid's TDS and the supplier's guidance. Cobalt in the fluid and corrosion at the edge must be confirmed by laboratory analysis; colour is a starting point, not a verdict. For tools whose edge quality bears on safety, such as medical or aerospace tools, do not release on floor judgement alone; get the quality engineer to confirm.

Cobalt is the biggest safety issue in this problem. A study reporting lung disease cases among carbide grinding workers notes that the cases came from the area with the lowest airborne cobalt, where the cobalt was dissolved in the coolant in ionic form, and names a coolant that dissolves less cobalt and effective exhaust as remedies (Sjögren et al., 1980). Wet carbide grinding without local exhaust has been reported to cause harmful cobalt exposure, and another survey found most airborne cobalt to be water-soluble ionic cobalt and recommends enclosing grinders and fitting local exhaust (Lichtenstein et al., 1975; Linnainmaa et al., 1996). The International Agency for Research on Cancer classified cobalt metal with tungsten carbide as probably carcinogenic to humans (IARC, 2006).

Metalworking fluids can harm health in their own right through skin contact and breathing in mist, so follow the SDS for gloves, eye protection and respiratory protection where needed, and take special care to keep reddened fluid and sludge off the skin (OSHA, n.d.). Removed sludge and spent fluid carry cobalt, so do not pour them down the drain; dispose of them under local rules.

Sources

  1. Atkins, P., & de Paula, J. (2014). Atkins' physical chemistry (10th ed.). Oxford University Press.
  2. Greenwood, N. N., & Earnshaw, A. (1997). Chemistry of the elements (2nd ed.). Butterworth-Heinemann.
  3. Human, A. M., & Exner, H. E. (1997). The relationship between electrochemical behaviour and in-service corrosion of WC based cemented carbides. International Journal of Refractory Metals and Hard Materials, 15, 65–71. https://doi.org/10.1016/S0263-4368(96)00014-5
  4. International Agency for Research on Cancer [IARC]. (2006). Cobalt in hard metals and cobalt sulfate, gallium arsenide, indium phosphide and vanadium pentoxide. IARC Monographs on the Evaluation of Carcinogenic Risks to Humans, Vol. 86.
  5. Irani, R. A., Bauer, R. J., & Warkentin, A. (2005). A review of cutting fluid application in the grinding process. International Journal of Machine Tools and Manufacture, 45(15), 1696–1705. https://doi.org/10.1016/j.ijmachtools.2005.03.006
  6. Lichtenstein, M. E., Bartl, F., & Pierce, R. T. (1975). Control of cobalt exposures during wet process tungsten carbide grinding. American Industrial Hygiene Association Journal, 36(12), 879–885. https://doi.org/10.1080/0002889758507360
  7. Linnainmaa, M., Kangas, J., & Kalliokoski, P. (1996). Exposure to airborne metals in the manufacture and maintenance of hard metal and stellite blades. American Industrial Hygiene Association Journal, 57(2), 196–201. https://doi.org/10.1080/15428119691015142
  8. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids
  9. Sjögren, I., Hillerdal, G., Andersson, A., & Zetterström, O. (1980). Hard metal lung disease: Importance of cobalt in coolants. Thorax, 35(9), 653–659. https://doi.org/10.1136/thx.35.9.653
  10. Stebbins, A. I., Horstman, S. W., Daniell, W. E., & Atallah, R. (1992). Cobalt exposure in a carbide tip grinding process. American Industrial Hygiene Association Journal, 53(3), 186–192. https://doi.org/10.1080/15298669291359492
  11. Tarragó, J. M., Fargas, G., Jimenez-Piqué, E., Felip, A., Isern, L., Coureaux, D., Roa, J. J., Al-Dawery, I., Fair, J., & Llanes, L. (2014). Corrosion damage in WC–Co cemented carbides: Residual strength assessment and 3D FIB-FESEM tomography characterisation. Powder Metallurgy, 57(5), 324–330. https://doi.org/10.1179/1743290114Y.0000000115
  12. Zhang, H. Q., Jia, X. M., & Wang, F. (2009). Study of inhibition function of grinding fluid additive to leaching cobalt from cemented carbide. Key Engineering Materials, 416, 381–385. https://doi.org/10.4028/www.scientific.net/KEM.416.381
  13. Zhang, H. Q., Jia, X. M., Gao, Y., & Hou, S. X. (2006). Study of inhibition to leaching of cobalt from cemented carbide tools. Key Engineering Materials, 315–316, 546–550. https://doi.org/10.4028/www.scientific.net/KEM.315-316.546
  14. Zhang, X. L., Jia, X. M., & Lian, J. X. (2010). Study on the mechanism of the cobalt leaching of cemented carbide in triethanolamine solution. Advanced Materials Research, 97–101, 1203–1206. https://doi.org/10.4028/www.scientific.net/AMR.97-101.1203
  15. Zheng, Y., Fargas, G., Armelin, E., Lavigne, O., & Llanes, L. (2019). Corrosion-induced damage and residual strength of WC-Co,Ni cemented carbides: Influence of microstructure and corrosion medium. Metals, 9(9), 1018. https://doi.org/10.3390/met9091018

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.