KALTECKOREA

BlogApplication notes

Why do hot melt bonds fail in hot warehouses and transit?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Adhesives

Switching to a hot melt with a higher softening point is the usual response when bonds fail in summer, but softening point does not tell how long a bond will carry a load in the heat, so failures can return after the change. What actually lies behind them can be low heat resistance, creep in the heat, a sustained load, unsuited packaging or the wrong adhesive amount, and sometimes two or more at once.

Background

Unloading pallets in a warehouse in midsummer, you find the flaps lifted on cases in the top tiers. From the far end of an export container comes word that a few cases have opened and spilled their contents. These are bonds that passed the sealing check inside the plant. Repacking, returns and reshipping, and damaged contents all cost money, and when cases open in a tall pallet stack the load can lean or collapse.

A hot melt is a thermoplastic resin applied molten that bonds as it cools and sets. Needing no time for solvent or water to leave, it suits fast packaging lines, but it keeps the property of softening when reheated, and limited heat resistance has long been named as its weakness (Li et al., 2008). Even set hot melt is a polymer, so under load it deforms little by little over time, and the same deformation happens far faster when the temperature rises (Ferry, 1980).

So there are two ways a bond fails in the heat. The adhesive itself softens or flows and lets go of the load, or the grip on the board surface was weak from the start and the bond comes apart at that boundary once heat and load are added. One symposium paper points out that storage temperatures sit well below a hot melt's softening point, yet adhesive properties can change greatly in between, so judging high-temperature bond strength from softening point and viscosity alone is easily wrong (Ambrosini, 1993).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the failed flaps, see which surface the adhesive stayed on, log when and where each failure happened, and compare the heat resistance in the hot melt's technical data sheet, the TDS, with the actual temperatures in the warehouse and in transit.

Hypothesis 1: low heat resistance

This hypothesis comes up first when a general-purpose hot melt chosen with indoor distribution in mind is used unchanged for summer logistics or export routes. The same goes for the time right after a change of supplier or grade to cut cost, a new route to a tropical region, and warehouses where cases sit for long in high tiers just under the roof. Think of a case sealing line that ran without trouble all spring. Once the rainy season ends and the heat sets in, flaps start lifting on cases in the upper tiers, and on the failed flaps the adhesive bead has split, half on each face, and a fingernail pressed into it leaves a mark.

How well a hot melt stands up to heat is set by the base polymer, the resin added for tack and the wax, and how they are blended. In a study of hot melts made from ethylene vinyl acetate copolymer, EVA, blended with aromatic hydrocarbon resins, lap-shear strength rose as the softening point of the added resin rose (Park & Kim, 2003). The standard test for the limit in the heat puts a fixed shear load on bonded specimens and raises the oven temperature in steps to find the temperature at which they fall. This heat-fail temperature marks a ceiling above which a bond under load should not be used, and in the round-robin of the same standard the EVA samples averaged a little over 60 °C, while polyamide and polyester samples came in at around 120 °C (ASTM International, 2015). As the adhesive nears this temperature, the solid mass softens and can no longer carry the load, and the adhesive layer then tends to split within itself rather than come away from the board.

Start the check with temperature records. Put temperature loggers in the upper tiers of the warehouse and inside containers, measure the midsummer peak, and compare it with the heat resistance or heat-fail temperature in the TDS. In a study that instrumented international container shipments, the highest temperatures came not while moving but while the containers stood at the docks, so the record must cover the waiting time in port too (Singh et al., 2012). Look also at whether the adhesive stayed split on both faces of the failed bond. Then make specimens from the board actually in use with the same hot melt, load them as the standard does, and measure the temperature at which they fall while the oven is raised in steps.

If the recorded peak reached the adhesive's limit, choose the grade again. Do not choose from the softening point figure alone; test whether a product holds at the recorded peak with the real board and the real flap load, and use one with margin. A new grade brings a different application temperature and viscosity, so set the tank and hose temperatures to the new TDS. On the warehouse side, revise stacking positions and ventilation so cases do not sit long in the tiers just under the roof.

Hypothesis 2: creep in the heat

Look at creep when flaps lift little by little over days or weeks at temperatures well below the adhesive's heat-fail temperature. Typical cases are long sea legs, stock held in the warehouse all summer, and cases stacked against a sunlit wall. A case whose flaps were firmly bonded at the final check before dispatch arrives a few weeks later with the flap edge open wide enough to admit a finger. The adhesive bead still joins both faces, but it has drawn out like thread and slid from where it was applied towards the flap edge.

Creep is the growing extension of a polymer held under a constant load as time passes. The polymer chains slip and rearrange bit by bit in the direction of the load, and the speed at which they move depends strongly on temperature, so raising the temperature has the same effect as running the clock faster (Williams et al., 1955; Ferry, 1980). That is why a flap load a bond would carry for months at room temperature can be lost in days in a hot container. A hot melt keeps its shape without a chemically linked network, relying on chain entanglements, small crystals and hard resin components, so as the temperature rises this hold loosens gradually and the adhesive can flow slowly even well below its softening point (Pocius, 2012). A bond lost to creep therefore tends to leave signs of stretching and sliding rather than a sudden break.

Creep only shows when watched over time. Draw a pen line across the flap edge and the edge of the bead on a few sealed cases, send them through the same warehouse and route, and see how far the lines have parted. In the laboratory, hang a constant load like a flap's on specimens made from the real board and measure the time to failure at the recorded warehouse temperature and at a few higher ones. The high-temperature stress test drawn up by the adhesion committee of a packaging professionals' body works in the same way, holding loaded bonds in an oven at a constant temperature for a long period (Ambrosini, 1993). If bonds fail with time at temperatures below the adhesive's heat-fail temperature, the cause leans towards creep.

If creep is the cause, review with the supplier a change to a grade that holds longer under load, and pick candidates by whether they last, in the oven load test above, at the recorded peak for the length of storage. Cutting the time spent in the heat works the same way. Avoid storage in the tiers under the roof and against sunlit walls, and move items with long container waits or warehouse stays up the dispatch order.

Hypothesis 3: sustained load

A case flap does not rest after it is bonded. Corrugated board tries to spring back open at the score, tightly packed contents push the flaps up, and cases stacked high bulge at the sides under the weight above, prying the bonds apart. Look at this hypothesis when a pack change puts more contents into the same case, when board arrives with shallow scores, or when pallets start being stacked one tier higher. A typical case: with the same hot melt and the same board, only the cases of a heavy item fail while those of a light item hold. On the failed cases the flap springs straight up as soon as the hand is lifted.

The forces on a packaging bond do not divide neatly into the single-direction shear or peel of a test machine. A paper on high-temperature stress resistance treats it as especially important for flaps with strong spring-back and for goods stored or shipped warm, and treats the size of the stress as a factor that changes high-temperature bond performance (Ambrosini, 1993). A springing flap applies a peel-type force that tries to lift the bond from its edge, and in peel the force concentrates on a narrow line at the very edge rather than spreading over the whole bond, so the same adhesive lets go at a far smaller force than in shear (Pocius, 2012). While this force acts day and night and the heat softens the adhesive, an opening that starts at the edge advances inward bit by bit, like a zip coming undone.

Gauge the size of the load first. Close an unbonded flap and let go to see how far it springs, and compare the depth of the scores with the board specification. Sort the failed cases by item, fill height and stack tier to see whether they cluster in heavy items or lower tiers. In the laboratory, put different loads on identical bonds in an oven at the same temperature and confirm whether heavier loads fail sooner.

If the load turns out to be the problem, reduce the force before changing the adhesive. Match fill height and case size so the contents do not push on the flaps, and agree a revised specification with the supplier for board with shallow scores. Set the length or time of the compression section so it holds the flaps until the adhesive has set enough. If force still remains, choose a grade strong in hot peel by testing it at the real load, and review the pallet stack height as well.

Hypothesis 4: unsuited packaging

Suspect the packaging when the board supplier has changed, when cases have moved to premium print with varnish or coating on the outer face, or when board with a high recycled fibre content or a moisture-barrier coating has come in. The same hot melt now meets a different surface. Suppose summer returns rose from the month after a change of board supplier. On the failed flaps the adhesive bead sits whole on one face, and the opposite face is smooth and shiny with almost no paper fibre on the bead.

A hot melt bonds by flowing, while molten, into the roughness and between the fibres of the board surface and setting there. A study comparing hot melt joints between pilot-made cartonboards found that the real contact area governed joint strength, and joints were stronger when the adhesive was applied first to the rougher board and the smoother board was pressed on. The same study reports that roughness depended mainly on whether the board was pigment coated, and that strong joints failed with fibre tear while weak joints mostly failed at the boundary between board and adhesive (Korin et al., 2012). An earlier paper from the same group also found that board roughness strongly affects hot melt joint strength (Vähä-Nissi et al., 2009). Surfaces carrying varnish, coatings or release agents, and plastic films, are smooth and hard to wet, so they need an adhesive made for that surface (Petrie, 2007). A bond weakly held at the boundary is the first to come apart there when heat softens the adhesive and load is added.

The clue lies on the failed surfaces. If the adhesive stayed cleanly on one side with no fibre on the other, the bond failed at the boundary; if torn fibre covers the whole bead, the grip between adhesive and board was enough. Sort failed cases by board lot and supplier, apply the same hot melt under the same conditions to the new and the previous board, and put both side by side in the same oven load test. Pull bonds apart by hand at room temperature as well and see how much fibre tears.

With the cause narrowed to the packaging, decide which side can change. For printed cases, agree the print specification with the board supplier so that no varnish or coating goes on the area where the flaps bond. If the board cannot change, pick a grade made for coated board through the same test. Where the two faces differ in roughness, moving the application so the adhesive goes on the rougher face first is worth a trial. When new board comes in, put it through a high-temperature stress test with the real hot melt before full production.

Hypothesis 5: wrong adhesive amount

The amount goes wrong when part of a nozzle clogs, when bead width or dot size is cut to save cost, or when the line speed goes up for more output while the applicator timer stays the same. The opposite happens too: more adhesive is applied in the belief that more is better, but the compression time is not changed. In the summer peak season the line speed goes up a step, and from that week flaps begin to fail. Opened cases show beads shorter and thinner than before, and in places the bead has broken up into dots.

A hot melt sets by cooling, so from the moment it is applied it loses heat to the board and the air (Li et al., 2008). A thin bead cannot hold its heat for long and tends to skin over before the opposite flap meets it, so it cannot flow in between the fibres and the real contact area shrinks. Given that contact area governs joint strength, a bond short of adhesive meets the heat with little margin from the start (Korin et al., 2012). A bead that is too heavy stays molten inside for longer, so when compression ends it takes the flap's spring-back while not yet set. The paper on high-temperature stress resistance also treats the amount of adhesive as a factor that changes high-temperature performance (Ambrosini, 1993).

Weighing makes the amount clear. Weigh the same case before and after gluing, or run paper under the nozzle and weigh one shot, and compare with the supplier's recommended amount. Inspect bead length, width and breaks by eye, and check that each nozzle delivers the same amount. Check against the records whether tank, hose and nozzle temperatures match the application temperature in the TDS, and whether the applicator timer and compression time were reset after the line speed changed.

If the amount was off, settle the amount that holds through a high-temperature stress test on the real board and control it by weight. Clean the nozzles and change filters at fixed intervals, and link the applicator timer to the line speed so bead length does not change with speed. If the amount goes up, reset the compression time to match.

Finding the cause

There is no need to test all five at once. Start with what the records can rule out. Compare warehouse and container peaks with the TDS, and set the dates when board supplier, print specification, pack size, line speed or hot melt grade changed against the date the failures began. The adhesive amount can be weighed without stopping the line. Oven load tests come after that.

The failed surfaces say the most. If the adhesive split and stayed on both faces, the adhesive itself could not stand the heat, so look at heat resistance and creep. If bonds failed all together around the midsummer peak, suspect heat resistance; if they failed after long storage below the heat-fail temperature, with signs of stretching and sliding, suspect creep. If the adhesive stayed cleanly on one face with no fibre, suspect the packaging surface or too little adhesive; if torn fibre covers the whole bead, the grip was enough and the board gave way first (Korin et al., 2012). Failures confined to heavy items or lower tiers point to a sustained load.

If that still does not settle it, run control trials that change one thing at a time. Put two hot melt grades on the same board, the same hot melt on the previous and the new board, different loads on identical bonds, and different amounts under otherwise identical conditions into the same oven. Before testing, bring cases and board to temperature and humidity in a standard conditioning atmosphere for package testing. Corrugated board changes its properties with temperature and humidity, so without conditioning the comparison wobbles (ASTM International, 2022). Set the oven to the recorded peak, make several specimens of each, and log both the number that fail and the time taken.

The final check happens on the real route. Send cases sealed under the changed conditions, with a temperature logger, through the same warehouse and route, and look at the flaps on arrival together with the peak temperature along the way. Count returns or repacks on the same basis as the previous summer, and the job is done only when that figure has come down.

The hypotheses often overlap. A bond short of adhesive, or one made on smooth board, has little margin from the start and fails with only a little more heat and load. Raising only the heat-resistance grade then tends to look ineffective. So put right first what the line and purchasing can fix, such as amount, compression and board surface, and on top of that choose a grade suited to the heat and to creep. In every case, the less load on the flap, the more margin there is.

Limits and cautions

Application temperature, adhesive amount, compression time and heat resistance differ by grade, equipment and board, so numeric decisions follow the hot melt's TDS and the equipment supplier's guidance. Softening point and heat-fail temperature are values for comparison and do not replace a test with the real board and the real flap load. For food, medicines and other goods under packaging rules, confirm compliance with the supplier and the quality engineer before changing adhesive, and judge any risk of a stack collapsing together with logistics and safety staff.

Safety matters too. Molten hot melt does not come off skin easily and can leave deep burns, so when handling tanks and nozzles follow the product's safety data sheet, the SDS, wear heat-resistant gloves and eye protection, and open a clogged nozzle only after releasing the pressure and lowering the temperature. An overheated tank gives off fumes and odour, so keep the area ventilated.

Sources

  1. Ambrosini, M. J. (1993). Heat-stress resistance of hot melt adhesives. In 1993 Hot Melt Symposium proceedings. TAPPI Press. https://imisrise.tappi.org/TAPPI/Products/HM/HM93119.aspx
  2. ASTM International. (2015). ASTM D4498-07(2015), Standard test method for heat-fail temperature in shear of hot melt adhesives. Withdrawn 2021. https://store.astm.org/d4498-07r15.html
  3. ASTM International. (2022). ASTM D4332-22, Standard practice for conditioning containers, packages, or packaging components for testing. https://store.astm.org/d4332-22.html
  4. Ferry, J. D. (1980). Viscoelastic properties of polymers (3rd ed.). Wiley.
  5. Korin, C., Seppänen, R., Vähä-Nissi, M., & Hallbäck, N. (2012). Influence of surface treatments on the mechanical strength of hotmelt adhesive joints made of cartonboards. Journal of Adhesion Science and Technology, 26(20–21), 2339–2356. https://doi.org/10.1163/156856111X599490
  6. Li, W., Bouzidi, L., & Narine, S. S. (2008). Current research and development status and prospect of hot-melt adhesives: A review. Industrial & Engineering Chemistry Research, 47(20), 7524–7532. https://doi.org/10.1021/ie800189b
  7. Park, Y.-J., & Kim, H.-J. (2003). Hot-melt adhesive properties of EVA/aromatic hydrocarbon resin blend. International Journal of Adhesion and Adhesives, 23(5), 383–392. https://doi.org/10.1016/S0143-7496(03)00069-1
  8. Petrie, E. M. (2007). Handbook of adhesives and sealants (2nd ed.). McGraw-Hill.
  9. Pocius, A. V. (2012). Adhesion and adhesives technology: An introduction (3rd ed.). Hanser.
  10. Singh, S. P., Saha, K., Singh, J., & Sandhu, A. P. S. (2012). Measurement and analysis of vibration and temperature levels in global intermodal container shipments on truck, rail and ship. Packaging Technology and Science, 25(3), 149–160. https://doi.org/10.1002/pts.968
  11. Vähä-Nissi, M., Korin, C., Seppänen, R., Laine, C., & Hallbäck, N. (2009). Influence of paperboard on bond formation and strength of adhesive joint. In 12th European PLACE Conference 2009 (Vol. 2, pp. 1743–1787). TAPPI Press.
  12. Williams, M. L., Landel, R. F., & Ferry, J. D. (1955). The temperature dependence of relaxation mechanisms in amorphous polymers and other glass-forming liquids. Journal of the American Chemical Society, 77(14), 3701–3707. https://doi.org/10.1021/ja01619a008

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.