KALTECKOREA

BlogApplication notes

Why does in-service hydraulic oil keep losing viscosity?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Equipment/Service Lubricants

Replacing the whole charge is the usual response when hydraulic oil loses viscosity, but without knowing what pulled the viscosity down, the same thing can happen again in the new oil, or money can go on replacing oil that was fine. What actually lies behind it can be a viscosity index improver cut by shear, thinner oil mixed in at top-up, solvent or fuel that got in, oil broken down by heat, or measurements made under different conditions, and sometimes two or more at once.

Background

With every routine oil analysis report, the kinematic viscosity at 40°C comes in a little lower. At first it is put down to scatter, but a few reports later the gap from the new-oil value is plain to see, and the people running the machines start to say the cylinders are slower than before or the oil runs hotter on summer afternoons. Whether to change the oil, or what to fix, is not clear.

Viscosity underpins everything hydraulic oil does. When it falls, internal leakage through the narrow gaps in pumps, valves and cylinders grows, so less flow is delivered at the same speed, and the oil film that keeps moving surfaces apart gets thinner. In hydraulic dynamometer tests, both the temporary thinning during running and the viscosity lost for good were linked to flow losses (Michael et al., 2018). The results show up as slower motion, more heat and faster wear.

A hydraulic oil's viscosity grade is set by the midpoint of its kinematic viscosity at 40°C, and each grade allows 10% either side of that value (ISO, 1992). Viscosity depends strongly on temperature, so standard equations and charts are used to estimate viscosity at other temperatures from values measured at two temperatures (ASTM International, 2020a). A claim that viscosity has fallen therefore means something only when values measured at the same temperature by the same method are compared, and if it has fallen even then, something in the oil has changed.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: gather past reports into one table and check that test temperature, method and laboratory match, put the top-up, oil temperature and maintenance records for the same period alongside, and compare everything with the new-oil values in the oil's technical data sheet, the TDS.

Hypothesis 1: sheared VI improver

Start with this hypothesis on machines running a hydraulic oil containing a polymer viscosity index improver, a multigrade hydraulic oil made so that its viscosity changes less with temperature, through a high-pressure pump. The viscosity index is a number for how small that change with temperature is. Typical cases are construction machinery working where outdoor temperatures swing widely, injection moulding machines and presses with high-pressure piston pumps, and circuits that constantly create large pressure drops across relief or proportional valves. Take an excavator filled with a multigrade hydraulic oil for easier winter starts. The report just after the change matched the new-oil value, but a few hundred hours later, with no top-ups and no change in smell or colour, the viscosity alone sits visibly below the new-oil value.

A viscosity index improver is a long polymer chain dissolved in the base oil. These long chains thicken the oil, but when they are forced at speed through the narrow gaps of pumps and valves under a large pressure drop, chains are stretched and broken, and the shorter pieces lose part of their thickening power. Multigrade hydraulic fluids are known to lose viscosity in service, by an amount that depends on the polymer's molecular weight and structure, the circuit's pressure drop and design, and the oil temperature; a higher molecular weight gives more thickening power but usually less resistance to shear (Hyndman et al., 2001). Loss from broken chains does not come back and is called permanent viscosity loss; separately, at high shear rates the chains merely line up with the flow and the oil thins temporarily, and the shares of the two losses shifted as service went on (Michael et al., 2018). Breaking chains creates no new light components, so this decline shows as viscosity alone going down, with no change in smell or flash point.

First check the TDS to see whether this is a multigrade hydraulic oil and whether it states a post-shear viscosity. That value may come from a test that shears a sample with ultrasound and measures the viscosity left, which has been reported to correlate well with shear degradation in a vane pump test (ASTM International, 2024b). If the in-service viscosity at 40°C has levelled off near that post-shear value, shear is a fair suspect. Work out the viscosity index as well. The improver is what lifts the viscosity index, so when it is cut, the viscosity index should move down along with the 40°C viscosity, while the flash point should stay close to the new oil's.

If shear is confirmed, getting the oil choice right is the key. Check whether the post-shear viscosity stays above the minimum set by the machine maker, and if it falls short, review with the supplier an oil with better shear stability or one grade higher. If a relief valve setting or an unnecessary throttle keeps creating a large pressure drop, fix the circuit as well. If viscosity has already settled at its floor, shear alone may not be a reason to rush an oil change, so time the change against the machine's viscosity limit and the other analysis results.

Hypothesis 2: thinner oil topped up

Suspect mixed oil on machines that are topped up often, at sites where several machines share one top-up container, and around a change of supplier or grade. A machine topped up every week because of a leak can have a sizeable share of its tank replaced by top-up oil within a few months. The same applies when thin flushing oil was not fully drained after a repair. On the shelf of a plant's maintenance room stand several drums of hydraulic oil of different grades, and the top-up jug carries no label. Viscosity does not drop all at once but steps down a little with each top-up.

When two oils of different viscosity are mixed, the blend's viscosity lies somewhere between the two, closer to the thinner one the larger its share. A standard sets out how to estimate the viscosity of a blend from the viscosities of the two oils and their proportions (ASTM International, 2023b). The same standard states that the calculation may not suit products containing components whose flow properties change strongly with shear, such as viscosity index improvers. Since one grade allows 10% either side of its midpoint (ISO, 1992), a moderate share of oil one grade lower can take the blend below the lower limit of the original grade.

Open the top-up records first. If they do not show when, how much and from which drum oil was added, check the top-up containers and the drums on the shelf directly and note the grade and TDS viscosity of each. Then estimate the share of thinner oil from the volumes added and the tank capacity, and see whether the calculated blend viscosity matches the measurement. An elemental analysis showing whether the pattern of additive elements has shifted from the new oil helps judge whether another product has been mixed in.

Do not try to restore viscosity lowered by mixed oil by pouring in a thicker one. The viscosity may then look right, but the additive make-up and viscosity index stay out of line. If the grade's lower limit has been crossed, change the oil, and from then on set one top-up oil per machine, with matching labels on the tank filler and the top-up container. After flushing, drain the remaining flushing oil thoroughly and bring the first oil analysis forward.

Hypothesis 3: solvent or fuel

Check whether there is a way in for a liquid much thinner and more volatile than the oil. Typical routes are parts cleaned with solvent and fitted before they are fully dry, washing a machine down with solvent near the tank breather and mobile equipment where fuel and hydraulic oil containers are used interchangeably. Picture a machine topped up in a hurry on a rainy day from a can that had held diesel. At the next analysis the viscosity is visibly lower, and opening the tank cap releases an unfamiliar smell.

Fuels and solvents are far less viscous than oil, so even a small amount pulls the blend's viscosity down. The products covered by the blend viscosity standard include blends with fuel components such as kerosene (ASTM International, 2023b). Such components are volatile, so the blend gives off vapour that ignites at a lower temperature, which is why flash point testing is used to detect volatile material mixed into a less volatile one (ASTM International, 2026). Viscosity and flash point falling together signal more light components, a sign common to ingress and to thermal cracking, the next hypothesis.

Measuring flash point alongside viscosity is an easy first fork in the road. The standard for monitoring in-service oils in auxiliary power plant equipment includes hydraulic systems in its scope and refers to test methods for both viscosity and flash point (ASTM International, 2023a). If the flash point is clearly below the new-oil value, ask a laboratory to check the boiling distribution by gas chromatography for a component bunched in a particular boiling range, such as diesel or solvent. On site, look at smell, colour, the history of top-up containers, and how cleaning work and refuelling are routed.

Once ingress is confirmed, close the route in and change the oil. Volatile material mixed in does not cleanly leave the oil just because the oil is warmed, and oil with a lowered flash point raises the fire risk. Fit cleaned parts only once fully dry, do no solvent cleaning near the tank breather, and keep labelled containers for hydraulic oil only, apart from fuel containers. In the first analysis after the change, check viscosity and flash point together.

Hypothesis 4: thermal cracking

Even when the bulk oil temperature is normal, oil may be touching a very hot surface somewhere. Cases include an electric tank heater for winter starts left on without circulation, a tank or pipe run passing close to high-heat plant such as a melting or reheating furnace, and long high-temperature running with cooling lost. One example is a tank whose heater was left on all weekend, opened on Monday morning. The heater sheath is coated with a black, burnt film, and from about then the reports show viscosity and flash point falling together while the oil darkens.

When hydrocarbon oil is overheated, long molecules break into shorter fragments, and these lighter molecules lower the viscosity, raise volatility and pull down the flash and fire points (Eastman, 2015). The same source explains that when fragments recombine into heavier products they raise viscosity instead, so heat does not always lower viscosity. The thermal stability test for heat transfer fluids covers fluids with maximum bulk operating temperatures of 260 to 454°C and measures how much breaks down over a set temperature and time (ASTM International, 2020b). Normal hydraulic operating temperatures are far below this, so suspecting thermal cracking in a hydraulic circuit means looking for locally hot surfaces, such as a heater sheath or a spot beside high-heat plant, rather than at the bulk oil.

Inspect the heater, the tank bottom and the pipework near high-heat plant directly. Check for burnt film on the heater sheath and black deposits on the tank bottom, and how the heater is switched and whether it is interlocked with the circulation pump. In analysis, compare viscosity, flash point and colour with the new oil, and if the flash point has dropped, use a boiling distribution analysis to see whether lighter fragments than the original oil are spread across a wide range. Light fragments spread widely, rather than bunched in one range as with fuel or solvent, weigh towards thermal cracking.

With thermal cracking, the first thing to fix is the hot surface rather than the oil. Interlock the heater so it runs only while the circulation pump runs, review a heater with a lower surface temperature or indirect heating through a heat transfer medium, and shield or relocate tanks and pipes beside high-heat plant. Broken molecules cannot be put back together, so change oil whose flash point and viscosity are outside limits, and clean any tank holding burnt deposits before filling with new oil.

Hypothesis 5: test mismatch

It may be the number that changed, not the oil. This happens after a change of analysis laboratory, after bringing in a portable on-site viscometer or switching to an instrument using a different method, when reports mix values at 40°C and at 100°C, and when samples are measured or shipped while hot or foamy. Say a plant moved its oil analysis to another laboratory this year. From the first report of the new laboratory the viscosity sits a step lower, but after that it runs flat.

The reference method for kinematic viscosity times how long a set volume of sample takes to flow through a glass capillary at a fixed temperature (ASTM International, 2024a). Another method measures dynamic viscosity with a rotating cell and divides by density to get kinematic viscosity, and the standard also sets out a correction for bringing its results into line with the reference method (ASTM International, 2021). As noted above, viscosity depends strongly on temperature, so even a small error in test temperature changes the value. With a multigrade hydraulic oil, viscosity varies with shear rate, so methods measuring at low and at high shear give different values for the same oil (Michael et al., 2018).

Lay out the reports and mark when test temperature, method number, laboratory and instrument changed. If the bend in the viscosity trend coincides with one of those marks, suspect a measurement difference first. The surest check is to split one sample and measure it at the same time at the old and new laboratories, or with the portable viscometer and the reference method. Measuring new oil the same way alongside gives a baseline for comparison.

If a measurement difference is confirmed, the job is not to change the oil but to reconnect the trend. Fix one laboratory, method and test temperature for the future and write them into the contract or the sample request, and if a change is unavoidable, measure the same samples at both during an overlap period to leave a basis for linking the two sets of values. Draw samples from a set point while the machine is running, and send them once cooled and free of foam.

Finding the cause

The first thing to rule out is the test conditions. The check finishes on paper, and if it turns something up, the remaining hypotheses are judged on values re-measured under the same conditions. Next come the top-up records and a look at the containers, then items already on the report or easy to add, such as flash point and viscosity index, with boiling distribution and elemental analysis commissioned after that.

The shape of the decline points the way. A single bend on the day the laboratory or method changed, followed by a flat line, points to a measurement difference; a multigrade oil drifting down without top-ups towards the post-shear viscosity in the TDS points to shear of the improver; and a staircase that steps down with each top-up points to thinner oil mixed in. A sudden large drop on one day suggests a single slug of solvent or fuel, and a gradual fall tied to heater use or high-heat exposure suggests thermal cracking.

Flash point is a good way to split the hypotheses into two groups. If viscosity has fallen but flash point has not, the cause lies on the side where no light components were added, such as shear of the improver or a lower-grade oil mixed in. If flash point has fallen too, it lies on the side where light components increased, such as solvent or fuel ingress or thermal cracking, and these two are separated again by whether the boiling distribution is bunched in one range or spread widely.

If that still does not settle it, run comparison tests. Measure the same sample at two laboratories, send new oil for the sonic shear test to confirm its post-shear viscosity, and measure a sample drawn from the top-up drum on its own. Make one comparison at a time, and compare the results with new oil measured by the same method. After fixing the cause, watch over several reports from the same laboratory by the same method to see whether the trend has stopped.

The hypotheses can overlap. While a multigrade hydraulic oil loses viscosity to shear, frequent top-ups with another grade because of a leak lay a second decline on top of it, and a laboratory change blurs the shape further. In such cases, pin down the test conditions first, sort out the top-up oil next, and then compare the remaining decline with the shear stability data, because while measurement and top-ups are unsettled, changes in the oil itself cannot be separated out.

Limits and cautions

Viscosity grades, the minimum and maximum viscosity a machine allows, and oil change criteria differ by machine and oil, so numeric decisions follow the machine maker's standards and the oil TDS. Do not judge oil condition on viscosity alone; read it with other results such as acid number, water, cleanliness and flash point. Boiling distribution and elemental analysis are laboratory work, and their results should be interpreted with the laboratory or the oil supplier.

Oil whose flash point has dropped sharply carries a higher fire risk, so keep heat sources and sparks away and bring the change forward even while the cause is being found. When sampling, use the designated sampling point and protective equipment so that hot oil does not spray from a circuit under pressure and temperature, and follow the product's safety data sheet, the SDS. If fuel or solvent has got into the oil, consult the SDS for that component too. Dispose of waste oil under local rules.

Sources

  1. ASTM International. (2020a). ASTM D341-20, Standard practice for viscosity-temperature equations and charts for liquid petroleum or hydrocarbon products. https://store.astm.org/d0341-20.html
  2. ASTM International. (2020b). ASTM D6743-20, Standard test method for thermal stability of organic heat transfer fluids. https://store.astm.org/d6743-20.html
  3. ASTM International. (2021). ASTM D7042-21, Standard test method for dynamic viscosity and density of liquids by Stabinger viscometer and the calculation of kinematic viscosity. https://store.astm.org/d7042-21.html
  4. ASTM International. (2023a). ASTM D6224-23, Standard practice for in-service monitoring of lubricating oil for auxiliary power plant equipment. https://store.astm.org/d6224-23.html
  5. ASTM International. (2023b). ASTM D7152-23, Standard practice for calculating viscosity of a blend of petroleum products. https://store.astm.org/d7152-23.html
  6. ASTM International. (2024a). ASTM D445-24, Standard test method for kinematic viscosity of transparent and opaque liquids and calculation of dynamic viscosity. https://store.astm.org/d0445-24.html
  7. ASTM International. (2024b). ASTM D5621-24, Standard test method for sonic shear stability of hydraulic fluids. https://store.astm.org/d5621-24.html
  8. ASTM International. (2026). ASTM D93-26, Standard test methods for flash point by Pensky-Martens closed cup tester. https://store.astm.org/d0093-26.html
  9. Eastman Chemical Company. (2015). What is thermal degradation and how is it measured? Chemical Engineering. Retrieved November 2026. https://chemengonline.com/partner-content/what-is-thermal-degradation-and-how-is-it-measured
  10. Hyndman, C. W., Kinker, B. G., & Placek, D. G. (2001). The importance of shear stability in multigraded hydraulic fluids. In G. E. Totten, D. K. Wills, & D. G. Feldmann (Eds.), Hydraulic failure analysis: Fluids, components, and system effects (ASTM STP 1339, pp. 523–534). ASTM International. https://doi.org/10.1520/STP38299S
  11. International Organization for Standardization [ISO]. (1992). ISO 3448:1992, Industrial liquid lubricants: ISO viscosity classification. https://www.iso.org/standard/8774.html
  12. Michael, P., Cheekolu, M., Panwar, P., Devlin, M., Davidson, R., Johnson, D., & Martini, A. (2018). Temporary and permanent viscosity loss correlated to hydraulic system performance. Tribology Transactions, 61(5), 901–910. https://doi.org/10.1080/10402004.2018.1439210

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.