Why does reused hydrotest water go bad and smell within weeks?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Prevention

Changing the water or pouring in another dose of biocide is the usual response when reused test water goes bad, but if the microbes stuck to tank and pipe walls and the sludge on the bottom stay put, fresh water tends to go bad again. What actually lies behind it can be sulphate-reducing bacteria, chemicals diluted by untreated top-up water, oil and scale brought in on parts, chloride and solids building up, or warm, stagnant storage, and sometimes two or more at once.

Background

Test shops that pressure-test valves, pump casings, heat exchangers and small vessels one after another collect the test water in a storage tank and use it again and again. Water that was clear for the first few weeks turns cloudy one day, a rotten-egg smell rises when the tank lid is lifted, and black sludge covers the bottom. Changing the water and washing the tank take time and add waste water disposal costs, and parts tested in that water come out with rust or black stains inside and must be cleaned again. The test pump, the tank and the connecting pipework corrode too, and hydrogen sulphide, the source of the smell, is a safety matter for the people working there.

Water going bad means microbes are growing in it. Microbes do not just drift in the water; they attach to tank and pipe walls and to the sludge on the bottom and form a biofilm, a slimy layer they make themselves, and beneath it corrosion of the metal can start or speed up. Corrosion in which microbes play a part is called microbially influenced corrosion, and its mechanisms and diagnosis are still being researched (Little et al., 2020). In corrosion that follows hydrotesting, too, it is treated as the central mechanism (Javaherdashti & Akvan, 2017).

Unlike water used once and thrown away, reused water takes something new on board with every test. Oil and rust from the parts, top-up water added to replace what was lost, air and heat all build up, while the chemicals added at the start are diluted or used up accordingly. That is how water that was fine for a few weeks can turn at some point.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: build a tank log of when the tank was filled, how often and how much it was topped up, which chemicals went in and how much, the water temperature and the day the smell first appeared, then compare it with the conditions of use in the chemicals' technical data sheets, the TDS.

Hypothesis 1: sulphate reducers

When a rotten-egg smell and black sludge appear together, think first of sulphate-reducing bacteria. They settle in readily where sludge has built up on the tank bottom, where water has not been circulated for a long time, and in large tanks where the water near the bottom is rarely exchanged. Take a test shop on a Monday morning: the test pump, idle over the weekend, is started and the first water out is grey, cloudy and strong-smelling. Inside the valve bodies tested that day a black film is left that comes off on a cloth.

These bacteria use sulphate in the water, where there is no oxygen, to break down organic matter or hydrogen, and release hydrogen sulphide as a result. Hydrogen sulphide meets iron to form black iron sulphide, and anoxic environments rich in sulphate are known to be especially corrosive (Enning & Garrelfs, 2014). Even when the upper water in the tank still holds oxygen, the inside of the sludge and the area beneath slime made by oxygen-using microbes stay out of its reach, so these bacteria can live there (ASSDA, 2010). The rotten-egg smell can be noticed at very low concentrations of hydrogen sulphide, but at higher concentrations the sense of smell is lost within minutes (OSHA, n.d.).

A smell is a clue, not a measurement. Take water separately from near the top of the tank and near the bottom, and scrape samples of bottom sludge and wall film as well. Field methods for estimating bacterial numbers, including bacteria living attached to walls, are set out in a standard test method, and since the condition of the bacteria can change while samples travel, analysis should start on site where possible (NACE International, 2014). The standard method that counts sulphate-reducing bacteria alone dilutes the sample into culture tubes and counts those that form a black precipitate, so the result takes several weeks to read (ASTM International, 2019).

Once sulphate-reducing bacteria are confirmed, changing the water alone is not enough. Empty the tank, remove the bottom sludge, wash the film off the walls and the connecting pipework with brushes or high-pressure water, and only then refill. Agree the biocide type, concentration and contact time with the supplier, and after refilling sample the same places at set intervals to see whether bacterial numbers climb again.

Hypothesis 2: untreated top-up

The water lost with each test, left in parts or spilled, is usually made up from the nearest mains or process water supply. If no chemical goes in with this top-up water, the inhibitor and biocide added at the start are diluted a little more with each top-up. It is easily missed when operators change and the top-up record breaks off, or when the level is simply brought back up without measuring the amount. Picture a test shop that metered chemicals in when the tank was first filled, but for the three months since has topped up with plain water from a hose whenever the level dropped. The water was fine for a while, and then one week it began to smell.

Chemicals only do their job at the set concentration. In one experiment, bacteria in a biofilm were killed about ten times less readily by the same biocide than bacteria floating in water, and a short dose at high concentration worked better than a long one at low concentration (Grobe & Stewart, 2000). Diluted biocide may leave the bacteria in such layers alive and linger only at a level that does not kill them, and one report found that such a sublethal biocide level actually encouraged biofilm growth and sped up corrosion of steel (Shi et al., 2025). A reactor experiment in which biofilms survived repeated biocide doses and still caused localised corrosion also shows that holding the dose may not be the whole answer (Jones et al., 2025).

Open the top-up log and work out the total top-up as a share of the tank volume. If the top-up has reached a sizeable part of the tank volume with no record of chemical being added, the concentration is already not what it was. Measure the inhibitor concentration by the method in the TDS, and run the residual test the supplier specifies for the biocide. Check in the log, too, whether the smell started soon after large top-ups.

If dilution is confirmed, treat the top-up water to the same concentration as the tank before it goes in. Meter the top-up volume and add chemical to match, and measure and record the concentration at set intervals. For the biocide, consider periodic doses at a concentration agreed with the supplier rather than a steady trickle at low level, and if a measurement falls below the limit, stop testing and correct it first.

Hypothesis 3: oil and scale

Testing parts without cleaning them, whether fresh from machining, delivered coated in rust preventive, or castings and forgings still carrying rust or mill scale, carries everything on them into the test water: cutting fluid, rust preventive oil, grease, grinding dust, sand and flakes of rust. The look is a rainbow film of oil floating on the water, and a brown-black mud that rises when the tank bottom is stirred with a pole. Bring up a scoop of that mud and it gives off the same rotten smell.

Oil is food for microbes. It has been shown that, even without oxygen, a range of microbes including sulphate-reducing bacteria can break down the saturated and aromatic hydrocarbons that make up oil (Widdel & Rabus, 2001). Settled scale and solids form a layer on the bottom, and beneath it oxygen cannot reach, so microbes grow well and under-deposit corrosion can occur on metal surfaces (Darwin et al., 2010). Sediment in test water can stay inside parts and cause crevice attack, so filtering the test water to remove undissolved solids is recommended (ASSDA, 2010).

The tank bottom and the water surface give the clues. Check for a floating oil film, measure the depth of the bottom layer with a pole, and filter a set volume of water through filter paper and dry what is left. Check in the work records how parts are cleaned before testing and which kinds arrive uncleaned. If the smell grows worse after days when oily parts were tested, the weight shifts to this hypothesis.

The first measure is to cut down what parts bring in. Degrease oily parts before testing, and knock off rust and scale before they go on the test bench. Fit the tank with a skimmer or absorbent pads for the oil film, put a strainer or filter ahead of the test pump, and draw off the bottom layer at set intervals. Avoid adding biocide alone while the oil on top and the mud below are left in place.

Hypothesis 4: chloride and solids

In a tank used for months without discarding any water, where evaporation and losses are made good with top-up water alone, the dissolved content keeps rising. It rises faster when the top-up is groundwater or water with salt in it, when parts that served at coastal sites come in, and when pickled or cleaned parts are tested without thorough rinsing. Look at a test shop whose tank stands in an open yard and has been topped up with groundwater all summer: the water looks clear, but tested parts show white salt marks once they dry.

When water evaporates only the water leaves, and the dissolved minerals stay behind in what remains, so the concentration rises with every round of evaporation and top-up. Cooling towers manage this build-up as cycles of concentration, the ratio against the make-up water, and set it by continuously measuring the conductivity of the circulating water (FEMP, 2011). Chloride makes water conduct well and hinders protective rust layers, so it increases the corrosion of steel (Revie & Uhlig, 2008). If sulphate builds up as well, there is more of the very material that sulphate-reducing bacteria use (Enning & Garrelfs, 2014).

A conductivity meter is enough to start. Measuring the conductivity of the tank water and the top-up water together and taking their ratio shows how many times more concentrated the tank has become, and measuring on the same day every week shows the trend. Measure chloride by titration or test strip, and total dissolved solids by evaporating a set volume of filtered water and weighing the residue. Check also whether parts tested in the tank water are left with white marks or salt crystals.

Once the build-up is confirmed, set a replacement limit for the tank water. When conductivity or chloride passes the set value, bleed off part of the water and replace it with clean water or change it all, and use low-salt mains or treated water for top-up. Rinse pickled or cleaned parts thoroughly before testing. If stainless steel parts are tested in the same water, set a stricter chloride limit than for carbon steel.

Hypothesis 5: warm stagnant tank

If the water spoils especially fast in summer, or starts to smell after a quiet spell with few tests, look at how it is stored. A black plastic tank in a sunny yard, a tank beside a boiler room or heat-treatment furnace, and periods when the water does not move for weeks, such as public holidays or slack months, all fall here. Consider a test shop with no tests scheduled for two weeks during the hot spell after the rainy season. When the pump is started again, the tank water smells far stronger than usual.

How fast microbes grow depends strongly on temperature. In a study that grew one species of sulphate-reducing bacteria between 12 and 48°C, the maximum growth rate was similarly high from 25 to 43°C and dropped sharply outside that range (Okabe & Characklis, 1992). Summer tank water can fall within that range. When water does not move, oxygen falls as microbes and corrosion consume it, an oxygen-free layer forms from the bottom up, and sludge settles and builds. Microbial corrosion has also been reported where raw test water was not fully removed from piping and a long delay followed before commissioning (ASSDA, 2010).

Measuring water temperature is the starting point. Record the temperature near the top and near the bottom of the tank in the morning and the afternoon, and look at the sun and any heat sources where the tank stands. Lay the test schedule beside the day the smell first appeared to see whether it began after a long period with the water standing still. If the smell and colour of top and bottom water differ greatly, the water is forming layers.

Changing the storage alone can change how long the water lasts. Move the tank into shade or indoors, or fit a sunshade cover, and keep it away from heat sources. Even when no tests are running, circulate the water with a small pump at set times to exchange the bottom water, and if a long shutdown is planned it is better to drain, wash and dry the tank and refill it afterwards.

Finding the cause

All five hypotheses lead to conditions in which microbes thrive, so finding one does not clear the rest. Go in order of what is easiest to measure. The tank log and top-up records, water temperature and conductivity can be put together within a day, and the oil film and bottom layer can be checked by eye and with a pole. Bacterial tests take time to give results, so take samples at the outset and run them alongside the other checks.

When the smell and colour began, and what they look like, give the direction. Black sludge and a rotten-egg smell point to sulphate-reducing bacteria; a smell that started after a large top-up points to diluted chemicals; a smell that worsened after oily parts were tested points to oil and scale coming in. Steadily rising conductivity and white marks on parts suggest accumulated chloride and solids, and water that spoils only in summer or after long idle spells suggests warm, stagnant storage.

If the causes do not separate, run a small comparison. Divide the same tank water between two or three clean containers, leaving one as it is, filtering and skimming another, and keeping a third somewhere cool, so only one thing differs at a time, then compare smell, colour and bacterial counts over several days. Putting identical carbon steel coupons in freshly treated and in old water and comparing the rust also helps.

The final check is the next cycle. After cleaning the tank and refilling it under the revised practice, measure bacterial counts, conductivity and chemical concentration at the same places and intervals, and compare how long it takes for the smell to appear with before. The cause has been found only when that period is clearly longer and tested parts come out with fewer stains.

Several hypotheses can also act together. With diluted biocide, oily mud on the bottom and summer temperatures all present, fixing just one lets the smell return quickly. In such cases, clean first, emptying the tank and removing sludge and film, then correct top-up treatment, oil control and storage in turn. Only once the places where microbes hide are gone can the effect of the other measures be compared fairly.

Limits and cautions

Biocide and inhibitor type, concentration, contact time and water replacement limits differ by chemical and by the material being tested, so numeric decisions follow each chemical's TDS and the supplier's advice. Bacterial counts alone do not prove microbially influenced corrosion; if parts or equipment have already corroded, send samples to a laboratory to analyse the corrosion products and the microbes together. Before disposing of treated or spoiled water, check the local discharge requirements.

Safety matters too. At high concentrations hydrogen sulphide can no longer be detected by smell, so never put your head into or enter a smelling tank or pit, and when cleaning an enclosed tank measure the gas level, ventilate and follow the confined space entry procedure (OSHA, n.d.). For biocides and inhibitors, follow the product's safety data sheet, the SDS, for protective equipment, and never mix different chemicals in one container.

Sources

  1. ASTM International. (2019). ASTM D4412-19, Standard test methods for sulfate-reducing bacteria in water and water-formed deposits. https://store.astm.org/d4412-19.html
  2. Australian Stainless Steel Development Association [ASSDA]. (2010). Hydrostatic testing of stainless steels. Australian Stainless, 47. https://assda.asn.au/blog/33-hydrostatic-testing-of-stainless-steels
  3. Darwin, A., Annadorai, K., & Heidersbach, K. (2010). Prevention of corrosion in carbon steel pipelines containing hydrotest water – An overview (Paper No. 10401). CORROSION 2010. NACE International. https://doi.org/10.5006/C2010-10401
  4. Enning, D., & Garrelfs, J. (2014). Corrosion of iron by sulfate-reducing bacteria: New views of an old problem. Applied and Environmental Microbiology, 80(4), 1226–1236. https://doi.org/10.1128/AEM.02848-13
  5. Federal Energy Management Program [FEMP]. (2011). Cooling towers: Understanding key components of cooling towers and how to improve water efficiency. U.S. Department of Energy. https://www.energy.gov/femp/articles/cooling-towers-understanding-key-components-cooling-towers-and-how-improve-water
  6. Grobe, K. J., & Stewart, P. S. (2000). Characterization of glutaraldehyde efficacy against bacterial biofilm (Paper No. 00124). CORROSION 2000. NACE International. https://doi.org/10.5006/C2000-00124
  7. Javaherdashti, R., & Akvan, F. (2017). Hydrostatic testing, corrosion, and microbiologically influenced corrosion: A field manual for control and prevention. CRC Press.
  8. Jones, L., Hanrahan, N., Salta, M., Skovhus, T. L., Thomas, K., Illson, T., Wharton, J., & Webb, J. (2025). Evaluating biocide efficacy in mixed-species biofilms: Insights from a dual anaerobic biofilm reactor. npj Materials Degradation, 9, 97. https://doi.org/10.1038/s41529-025-00628-0
  9. Little, B. J., Blackwood, D. J., Hinks, J., Lauro, F. M., Marsili, E., Okamoto, A., Rice, S. A., Wade, S. A., & Flemming, H.-C. (2020). Microbially influenced corrosion—Any progress? Corrosion Science, 170, 108641. https://doi.org/10.1016/j.corsci.2020.108641
  10. NACE International. (2014). NACE TM0194-2014, Field monitoring of bacterial growth in oil and gas systems.
  11. Occupational Safety and Health Administration [OSHA]. (n.d.). Hydrogen sulfide: Hazards. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/hydrogen-sulfide/hazards
  12. Okabe, S., & Characklis, W. G. (1992). Effects of temperature and phosphorous concentration on microbial sulfate reduction by Desulfovibrio desulfuricans. Biotechnology and Bioengineering, 39(10), 1031–1042. https://doi.org/10.1002/bit.260391007
  13. Revie, R. W., & Uhlig, H. H. (2008). Corrosion and corrosion control: An introduction to corrosion science and engineering (4th ed.). Wiley.
  14. Shi, X., Zhang, Y., Zhang, R., Li, C., Wang, C., Wang, X., Sand, W., & Duan, J. (2025). Sublethal THPS accelerates Pseudomonas-associated steel corrosion by stimulating biofilm development and microbial electron uptake. npj Materials Degradation, 9, 75. https://doi.org/10.1038/s41529-025-00625-3
  15. Widdel, F., & Rabus, R. (2001). Anaerobic biodegradation of saturated and aromatic hydrocarbons. Current Opinion in Biotechnology, 12(3), 259–276. https://doi.org/10.1016/S0958-1669(00)00209-3

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.