KALTECKOREA

BlogApplication notes

Why does stainless equipment pit at the welds after hydrotest?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Prevention

Stainless steel is thought not to rust, so the test water often goes unchecked or is left standing after the test, but the thin film that protects stainless steel can break down point by point in the face of chloride, crevices and microbes. What actually lies behind the pits can be chloride in the test water, microbes grown in standing water, chloride concentrated at the waterline, heat tint left on the welds, crevices under gaskets or iron contamination from carbon steel, and sometimes two or more at once.

Background

Stainless steel vessels and piping in 304L or 316L are hydrotested, and a few weeks or even months later, as start-up approaches, an inspection shows rows of pinpoint brown spots along the weld lines, some with red rust trails running down from them. Stainless steel was chosen because it resists corrosion and stays clean, so these spots are a quality problem in themselves, and once a pit goes through the wall the section must be cut out and rewelded. In food, pharmaceutical or water treatment plant, rust and the microbes in it can contaminate product and water. In one real case, 316L piping at a water treatment plant began leaking at circumferential welds about three months after hydrotest (Bedoya-Zapata et al., 2021).

Stainless steel does not rust because of an extremely thin passive film that chromium forms on its surface. When ions such as chloride break this film at one point, metal ions react with water inside that spot and make it acidic, chloride is drawn in, and the hole deepens by itself as a pit (Frankel, 1998). The stronger the chloride, the higher the temperature and the more crevices there are, the more easily this happens, and grades containing molybdenum hold out better. Welds differ from the parent metal in structure and surface, so they are places where the film is easily weakened (Sedriks, 1996).

A hydrotest can create all of these conditions at once. Case histories have been collected of stainless steel piping, storage tanks and heat exchangers suffering microbial corrosion from cooling water and hydrotest water, with the attack concentrated at the welds (Kobrin et al., 1997). The test itself may be over in a day, but what water went in, how long it stayed and how it was drained and dried decide the state of the surface in the weeks that follow.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: map the rust spots on the drawing, with photographs, as welds, waterline, gasket seats or bottom, and compare the test water source and its quality data, how long the water stayed in, the drain and drying records, and the purge gas and pickling records from welding against the test procedure and the specification.

Hypothesis 1: chloride-rich water

Chloride in the test water becomes a problem where no test water is specified and whatever water is to hand gets used. Plant well water, river water, process water and coastal groundwater with seawater mixed in are examples, and water heated during the test or warmed by summer sun raises the risk. Take the case of a 316L storage tank filled with the well water previously used to test carbon steel equipment. Looking inside months later, before the insulation comes off, rows of pinhole-like brown spots line both sides of the weld seams on the bottom and walls.

Each grade has a range of chloride concentration and temperature it can withstand, and the test water must be within it. Where contact is brief, such as 24 to 48 hours, that limit may sometimes be exceeded, but if the chloride content is unknown the water should be analysed (ASSDA, 2010). Higher chloride lowers the potential and temperature at which the film breaks down, so pitting starts more easily in the same grade (Frankel, 1998), and the first place is likely to be the welds, where the film is weakest. In the laboratory, the resistance of grades to pitting and crevice corrosion is compared by immersion in ferric chloride solution (ASTM International, 2020).

Finding the source of the test water and its certificate comes first. If there is none, take water from the same source and measure chloride by titration or by ion analysis in a laboratory, and confirm from the records the water temperature during the test and the number of days the water was in contact. Compare these values with the chloride limit in the owner's specification or the test procedure. If the spots are spread evenly over every weld that was under water, the weight shifts to this hypothesis.

Write the test water quality into the procedure as numbers. Use clean water such as demineralised water, steam condensate or treated mains water, and avoid raw water such as river or well water (ASSDA, 2010). Set the chloride limit, water temperature and maximum holding time to suit the grade, and drain and dry within that time once the test is done. Use water from carbon steel testing, or reused water, only after measuring its chloride and finding it within the limit.

Hypothesis 2: microbial attack

Microbes can grow while a system is left full after the test, or half drained, waiting for start-up. Typical cases are new plants with slipping schedules, tests run with unfiltered raw water, and piping where water stays at low points. A 316L piping system, for instance, stands for months with some water left in it after its test because start-up has been delayed. When the pressure goes up just before start-up, droplets form at several circumferential welds, and from outside the holes are no bigger than a pinpoint.

In a study of twelve pitted austenitic stainless steel welds, eleven showed microbial corrosion or attack in which microbes and chloride acted together, and welds that were not sensitised were attacked as well (Borenstein, 1988). In the water treatment plant piping mentioned above, the pits lay in the weld metal and heat-affected zone, wide cavities had formed beneath small surface holes, and structures consistent with sulphate-reducing and iron-oxidising bacteria were seen (Bedoya-Zapata et al., 2021). In another case, the rapid pitting failure of 304 pipework at a chemical plant was microbial corrosion brought on by poor-quality test water and uncontrolled test practice (Stott, 2022). Microbes attach to welds and build nodule-like deposits, beneath which a crevice forms with little oxygen and gathering chloride.

Examine the area round the spots first. Look for small brown or red nodules sitting over them, and if there are any, lift them off with a clean tool before scraping and send them to a laboratory as samples for microbial analysis. From the records, confirm when and how far the water was drained after the test and what kind of raw water was used. If a leaking weld can be cut out, section and polish it to see whether a wide cavity lies beneath a small opening.

If the evidence leans towards microbes, leaving no water is the key. Draining fully and drying straight after the test is the main way to prevent microbial corrosion, and it is recommended to finish preferably within 24 hours and certainly within 5 days (ASSDA, 2010). Unless the system goes straight into service, do not leave it full, and avoid leaving it partly drained. For a system that already carries deposits, remove them, clean it, and decide with a corrosion specialist whether to pickle and passivate again.

Hypothesis 3: waterline salts

Draining only part of the water, or leaving water in the bottom of horizontal vessels and tanks to dry slowly, lets evaporation gather salts. Outdoor equipment in the sun, tanks left with the manway open and warm seasons make it worse. Here is a storage tank half drained after its test and left for weeks with the manway open. On the inside wall, brown spots form a band along the level of the remaining water, while the submerged wall below and the dry wall above are clean.

Salts stay behind as water evaporates and gather in what remains, so even clean water can become a very strong and aggressive solution as it dries slowly. That is why partial draining is warned against as potentially very serious (ASSDA, 2010). Where the surface of the water meets the wall, the thin film dries first, so chloride tends to concentrate there, and stronger chloride reaches the conditions for breaking down the film more easily (Frankel, 1998). As the level falls and pauses, this repeats at each level, and several bands of spots can form.

Whether the spots form a horizontal band is the clearest sign. Check that the height of the band matches the level of water left after draining, and if there are dried droplet rings or white salt crystals on the bottom, swab them and test for chloride. If water is still standing, measuring its chloride and comparing it with the original test water shows how far it has concentrated.

The remedy starts with leaving no water. Drain completely, and rather than letting the last moisture evaporate on its own, wipe it out or blow it dry with dry air. If salt has already been left at the waterline, rinse with clean water and dry at once, and judge whether to restore the pitted areas by pickling and passivation. For large tanks, confirm at the design stage that the drain is placed so the bottom empties fully.

Hypothesis 4: heat tint left on

If the back of a weld was not covered with a purge gas such as argon during welding, or the gas ran short, heat tint is left inside the weld, an oxide discoloration that darkens from yellow through blue to black. Typical cases are circumferential site welds on piping, joints whose inside could not be reached for pickling, and joints where the purge gas supply ran out. Assume that on a day when 316L piping was being joined on site, the purge gas cylinder ran empty and a few joints were welded anyway. Through an inspection camera, a dark blue band shows round the root of those joints only, and the rust spots sit inside that band.

Beneath the oxide scale formed in welding lies a thin layer that has lost chromium, so to restore corrosion resistance this chromium-depleted layer must be removed along with the tint (TWI, n.d.). In a study of 304L and 316L weldments in fresh water containing microbes, corrosion nodules formed at crevices placed in heat-tinted areas, but on specimens whose tint had been removed chemically, electrochemically or mechanically, no nodules formed even under the same crevice conditions (Li et al., 1995). In the water treatment plant piping too, the pits gathered in heat-tinted areas left by missing or deficient purge gas during site welding (Bedoya-Zapata et al., 2021).

Look at the colour inside the welds and the width of the band with an inspection camera or mirror. If the spots gather inside dark tint bands and are almost absent on lightly tinted joints, they fit this hypothesis. Check in the welding records, joint by joint, whether purge gas was used, whether the oxygen content of the backing gas was measured, and whether the weld was pickled afterwards.

Heat tint should not be left in place. Pickling gives the best corrosion resistance, better still when preceded by grinding, while wire brushing and sand blasting are less effective because they generally do not remove the chromium-depleted layer (TWI, n.d.). In future welding, measure the oxygen content of the purge gas as work proceeds, set acceptable tint levels in the specification, and pickle or reweld joints that exceed them.

Hypothesis 5: gasket crevices

If the spots sit in a ring on a flange face or where a test blind was fitted, rather than at the welds, look at the crevice under the gasket. Temporary gaskets fitted for the test, fibre gaskets, blinds left in place after the test, threaded joints and the narrow gaps between lapped plates are such places. Picture a test blind being removed a few weeks after the test. On the flange face, brown spots run round the ring where the gasket sat, while the face outside it is clean.

Water inside a narrow crevice barely mixes with the water outside. Once the oxygen in the crevice is used up, the metal inside becomes the side that dissolves, the dissolved metal ions react with water and make the crevice acidic, and chloride from outside gathers inside to balance the charge, breaking down the film. So crevice corrosion starts at lower temperatures and chloride levels than pitting on an open surface of the same grade (Sedriks, 1996). Standard tests likewise fit a device that creates crevices on the specimen to assess crevice corrosion resistance separately (ASTM International, 2020).

The shape and position of the spots give the answer. See whether they lie inside the ring between the gasket's outer and inner diameters, and whether the same pattern appears at blinds or bolt washer seats. Confirm the gasket material and when it was removed after the test, and if the removed gasket is still available, check whether it was wet or stained with rust.

Crevices should be removed or kept short-lived. Take off temporary gaskets and blinds as soon as the test is over, rinse the flange faces with clean water and dry them, and choose gasket materials that do not soak up water for any that stay in place. Designing out crevices during fabrication is also recommended (ASSDA, 2010). Pitting on a flange face affects the flatness of the sealing surface, so judge whether it needs re-machining.

Hypothesis 6: iron contamination

Iron is transferred onto stainless steel surfaces when stainless is fabricated in the same shop as carbon steel, when grinding discs, wire brushes, tools and jigs used on carbon steel are shared, and when test water is fed through hoses and tanks used for testing carbon steel equipment. Think back to a stainless vessel assembled in a corner of a shop that builds carbon steel structures, with its weld beads dressed by the same grinder. A few days after the test, red rust stains have spread along the ground areas and the trails where test water ran down.

Iron embedded in or smeared on the surface is not stainless, so it rusts as soon as it gets wet, and that rust looks as if the stainless steel itself has rusted. The standard practice for stainless steel surface treatment treats such free iron, together with rust, scale and grease, as contamination that can impair metallurgical and sanitary performance (ASTM International, 2025). Where iron rust covers the surface, it can create crevice-like conditions on the stainless underneath and become a place where localised corrosion starts. A literature review of fabrication damage and iron contamination found that chemical surface treatments appeared always to be better than mechanical ones at restoring corrosion resistance (Coates, 1990).

Start by wiping the stains. If they come off easily with a non-abrasive cleaner and the surface beneath is sound, suspect surface iron first; if pits remain after cleaning, corrosion may have started underneath. Whether free iron is present is confirmed by standard methods such as wetting or high-humidity exposure and the copper sulphate test (ASTM International, 2025). Check, too, whether the rust stains follow grinder and tool marks.

When iron is the cause, restore the contaminated surfaces by pickling or passivation and test again to confirm no iron remains. From then on, keep dedicated discs, brushes and tools for stainless, separate the work areas, and do not share test equipment, hoses or water between carbon steel and stainless testing. Pad any points that rest on forklift forks or carbon steel supports.

Finding the cause

Sorting out six hypotheses does not need a laboratory at the start. The test water certificate, holding time, drain and drying records, and weld purge and pickling records can be checked on paper, and the position and form of the spots can be seen with an inspection camera and a torch. Chloride measurement and free iron tests can be done on site, with microbial analysis and sectioning after that.

Where the spots lie is the strongest clue. A horizontal band suggests chloride concentrated at the waterline, a ring at a gasket or blind suggests a crevice, and spots gathered inside dark tint bands suggest heat tint left on. Stains that wipe off and follow grinder marks point to iron contamination, and spots spread evenly over every weld that was under water send attention first to chloride in the test water. Nodules sitting on the spots, with cavities wider inside than the surface holes, call for laboratory analysis to check for microbial involvement.

If that still does not settle it, compare places within the same system that differ in one condition. Counting the spots side by side on pickled and unpickled joints, on sections drained at once and those left full, and on items that passed through carbon steel test equipment and those that did not shows what made the difference. If needed, immerse welded coupons of the same grade in the test water and change one condition at a time.

The final check is the next test under the revised procedure. After changing the test water quality, draining and drying, purge and pickling, and tool segregation, look at the same places after the same interval and compare the number of spots with earlier records on the same basis. The cause has been found only when no spots appear.

These hypotheses tend to overlap in the same place. Heat tint weakens the film, microbes in standing water build nodules and crevices over it, and chloride-rich water or concentration at the waterline makes the chloride in those crevices stronger. In such cases, put prompt draining and drying and the removal of heat tint right first, because without water neither chloride nor microbes can act, and an intact film leaves a margin to withstand the remaining conditions.

Limits and cautions

The chloride content and temperature allowed in test water for each grade, the maximum holding time and acceptable tint levels differ by design code, owner's specification and the guidance of steel and welding consumable suppliers, so numeric decisions follow those documents. How deep pits have gone into the wall and whether the equipment can stay in service are for a pressure equipment inspector and a corrosion specialist to judge, and microbial corrosion is confirmed by laboratory analysis.

Safety matters too. Acids and pastes used to pickle stainless steel can contain components that are highly harmful to skin and lungs, so follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and dispose of spent solution as required. Vessels purged or dried with nitrogen or argon can be short of oxygen inside, so ventilate them and measure oxygen before entry. When grinding pitted areas, guard against dust and noise.

Sources

  1. ASTM International. (2020). ASTM G48-11(2020)e1, Standard test methods for pitting and crevice corrosion resistance of stainless steels and related alloys by use of ferric chloride solution. https://store.astm.org/g0048-11r20e01.html
  2. ASTM International. (2025). ASTM A380/A380M-25, Standard practice for cleaning, descaling, and passivation of stainless steel parts, equipment, and systems. https://store.astm.org/a0380_a0380m-25.html
  3. Australian Stainless Steel Development Association [ASSDA]. (2010). Hydrostatic testing of stainless steels. Australian Stainless, 47. https://assda.asn.au/blog/33-hydrostatic-testing-of-stainless-steels
  4. Bedoya-Zapata, Á. D., Franco-Rendón, C. M., León-Henao, H., Santa, J. F., & Barrada, J. E. G. (2021). Failure analysis of a welded stainless-steel piping system with premature pitting. Engineering Failure Analysis, 119, 104986. https://doi.org/10.1016/j.engfailanal.2020.104986
  5. Borenstein, S. W. (1988). Microbiologically influenced corrosion failures of austenitic stainless steel welds. CORROSION 88. NACE International. https://doi.org/10.5006/C1988-88078
  6. Coates, G. E. (1990). Effect of some surface treatments on corrosion of stainless steel. CORROSION 90. NACE International. https://doi.org/10.5006/C1990-90539
  7. Frankel, G. S. (1998). Pitting corrosion of metals: A review of the critical factors. Journal of The Electrochemical Society, 145(6), 2186–2198. https://doi.org/10.1149/1.1838615
  8. Kobrin, G., Lamb, S., Tuthill, A. H., Avery, R. E., & Selby, K. A. (1997). Microbiologically influenced corrosion of stainless steels by water used for cooling and hydrostatic testing (IWC-97-53). 58th Annual International Water Conference, Pittsburgh. Nickel Development Institute Publication No. 10085. https://www.nickelinstitute.org/media/8daa62263c08cc8/10085_microbiologicallyinfluencedcorrosionofstainlesssteelsbywaterusedforcoolingandhydrostatictesting.pdf
  9. Li, P., Buchanan, R. A., Lundin, C. D., Tuthill, A. H., Avery, R. E., Angell, P., & Sachs, D. E. (1995). Effects of postweld treatments on corrosion of stainless steel weldments in microbial fresh-water systems. CORROSION 95. NACE International. https://doi.org/10.5006/C1995-95192
  10. Sedriks, A. J. (1996). Corrosion of stainless steels (2nd ed.). Wiley.
  11. Stott, J. (2022). Rapid pitting failure of Type 304 stainless steel pipework. Journal of Failure Analysis and Prevention, 22(6), 2462–2466. https://doi.org/10.1007/s11668-022-01545-z
  12. TWI Ltd. (n.d.). How do I remove heat tint formed during welding or improper heat treatment of stainless steels? Retrieved November 2026. https://www.twi-global.com/technical-knowledge/faqs/faq-how-do-i-remove-heat-tint-formed-during-welding-or-improper-heat-treatment-of-stainless-steels

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.