BlogApplication notes
Why does fog form inside insulating glass units?
- Type
- Application notes
- Published
- 23 November 2026
- Prepared by
- Jonghwan Moon
- Product group
- Sealants & Damping
Wiping the glass or ventilating the room is the usual response to fogged insulating glass, but when the fog is between the two panes, moisture or other substances have already got past the seal, and nothing done from outside will clear it. What actually lies behind it can be a broken or incomplete primary butyl seal, a weakened secondary sealant, a saturated desiccant, ingredients migrating from glazing materials, or water standing at the bottom of the frame, and sometimes two or more at once.
Background
On a cold morning, several office windows have gone cloudy. Wiping the room side changes nothing, nor does wiping the outside, and a closer look shows droplets and smears sitting between the two panes. Some units clear as the weather warms and fog again when it turns cold, while in others a white film stays even through the summer.
A unit fogged between the panes cannot be restored by wiping or drying, so the whole unit usually has to be replaced. Beyond the loss of view and appearance, in units filled with a gas such as argon, the fill also diffuses out through the edge seal and is diluted by air, so the poorer the seal, the more thermal and sound insulation fall (Wolf, 2002). For large units on upper floors, replacement brings equipment, labour and disruption for occupants with it.
An insulating glass unit holds two panes apart with a spacer and seals the edge so that the space between stays dry. In the dual-seal design widely used today, a primary seal of polyisobutylene, a butyl-type material, sits between spacer and glass to block water vapour and gas, and a secondary sealant such as polyurethane, silicone or polysulphide fills the perimeter outside it and holds glass and spacer together. Because of the difference in vapour pressure with the outside, water vapour seeps slowly into every unit, and the desiccant in the spacer takes it up until it is saturated, after which condensation forms between the panes (Van Den Bergh et al., 2013). That is why fogging between the panes under normal use is taken as the end of a unit's service life (Wolf, 2002).
In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: confirm that the fog really is between the panes, record the position, orientation and manufacturing marks of each fogged unit, and compare the glass manufacturer's glazing instructions with the actual frame drainage and the materials touching the unit.
Hypothesis 1: weak primary seal
When units fog soon after installation, suspect the primary seal as made in the factory first. Typical cases are butyl not applied evenly to the spacer, a bead that breaks at a corner, or too little pressing force or time after the panes are assembled, so that the butyl never fully wets the glass. On one site, only a few of the units delivered from the same factory in the same month fog in their first winter. Looking at a fogged unit's edge at an angle, the dark butyl line that runs evenly on the other units narrows and breaks off at one corner.
Moisture protection in an insulating glass unit rests almost entirely on the primary seal, because the water vapour permeability of a polyisobutylene primary seal is far lower than that of the secondary sealant, whether silicone, polysulphide or polyurethane. The primary seal must therefore be properly dimensioned, free of voids and fully wet both spacer and glass, and pressing is controlled to give a butyl layer 0.3 to 0.4 mm thick between spacer and glass with a vapour path about 5 to 6 mm long (Wolf, 2002). Moisture passing the primary seal rises as the butyl gap between spacer and glass gets wider and falls as the path gets longer, so a spot where too little butyl has shortened the path, or where the bead is broken, becomes a shortcut for vapour (Van Den Bergh et al., 2013). Moisture entering by that shortcut fills the desiccant sooner than planned, and once the desiccant is full, fog forms.
Looking at the glass edge at an angle shows the primary seal line. Compare fogged and clear units side by side to see whether the line runs at an even width along all four edges, and whether there are breaks, narrow spots or voids like bubbles. A suspect unit can be compared with a sound one by the standard test that measures the frost or dew point of the space between the panes (ASTM International, 2020b), and a removed unit can be cut at the edge to see how far the butyl wetted the glass. Group the fogged units by their manufacturing marks to see whether they cluster in one production lot.
Replace the fogged units, and once the cause is narrowed to the primary seal, ask the supplier for corrective action in production. Handing over photos, locations, manufacturing marks and cut sections together makes it easier for the supplier to check them against production records. Specify replacement units that have passed recognised performance tests such as the long-term moisture penetration test (CEN, 2018). At delivery, check the primary seal line on a sample of units.
Hypothesis 2: aged secondary seal
Look at the secondary sealant when the unit's edge takes a lot of sun and heat. Typical places are sloped glazing and rooflights where the frame does not cover the edge, tinted or solar-control glass, and south- and west-facing walls in hot regions, especially where the secondary sealant is an organic type such as polysulphide or polyurethane. Rooflights on a south-facing slope show the contrast. Units on the upper slope fog one after another within a few years, while the vertical windows of the same building are still clear.
The secondary sealant's job is less about keeping moisture out than about holding the glass and protecting the primary seal. In a dual seal, the secondary sealant's vapour permeability plays a small part in service life; what matters is how firmly it resists when rising temperature raises the pressure between the panes, because that sets how far the primary seal is pulled open. Even an edge hidden by the frame receives about 1 to 8% of incident sunlight through internal reflection in the glass, and the glass adhesion of organic sealants such as polysulphides and polyurethanes can be irreversibly destroyed by the short wavelengths between 280 and 380 nm. Water, high temperature and sunlight acting together put the greatest stress on the edge, and under them organic sealants fail progressively near the glass interface (Wolf, 2002). In one study of dual-sealed units held at 55 °C and 100% relative humidity for three months, units with a silicone secondary sealant showed the least water pick-up in the desiccant, and those with organic sealants about three times as much (Wolf, 1992).
The secondary sealant can be seen directly once a glazing bead is removed. Look for places lifted or detached from the glass, cracks, a tacky or chalky surface and uneven thickness, and push gently at the edge with a fingernail to see whether it is still bonded. Check against the location records whether fogged units cluster where edges are exposed, on orientations with long sun, or in tinted glass. Confirming the secondary sealant type from the unit manufacturer's data speeds up the judgement.
Shading the edge from sunlight is the first measure. Where edges are exposed, as in sloped glazing, cover the edge of organic sealants with strips, gaskets or tape, and where they cannot be covered, agree with the glass manufacturer on units whose secondary sealant suits those conditions. Replace fogged units, but change edge protection and sealant type at the same time, because the same unit under the same conditions will give the same result.
Hypothesis 3: saturated desiccant
When units installed at the same time in an older building fog one after another year by year, the desiccant may simply be full even without an obvious defect in the seal. In warm, humid climates and in buildings with high indoor humidity, such as swimming pools and kitchens, that point can come sooner. Classroom windows in an older school building are an example. A few more units fog every year, and the order is spread evenly across the building rather than clustered on one orientation or floor.
Moisture enters every insulating glass unit little by little. The desiccant extends service life by taking up this moisture and organic vapours in the space between the panes, but its capacity is limited, and vapour that seeps in once it is full condenses as fog on the inner faces. Units mostly use molecular sieve or a blend of molecular sieve and silica gel; a 3 Å molecular sieve takes up water vapour while excluding most other molecules, and silica gel, with its wide range of pore sizes, also captures organic compounds. Moisture can also be trapped between the panes during manufacture (Van Den Bergh et al., 2013). The European long-term test builds on this, calculating a moisture penetration index from the moisture taken up by the desiccant after set temperature and humidity conditions (CEN, 2018). While that standard was being developed, low temperatures did not cause failure, and sustained high humidity, rather than humidity cycling, was the main driver of moisture into the units (Wolf, 2002).
Measuring the dew point can catch a change before it shows. Measuring the dew or frost point of a few still-clear units by the standard test and comparing them with the value for new units picks out units whose dew point has risen before they fog (ASTM International, 2020b). Group fogged and clear units by installation year and manufacturing marks, and see whether fogging spreads with age or clusters in particular lots or positions. If no breaks or lifting are found in the seals and the fogging spreads evenly with age, this hypothesis remains.
A saturated unit has reached the end of its life, so plan replacement. Grouping units whose dew point has started to rise and replacing them together saves equipment and labour. Specify new units that pass recognised tests such as the long-term moisture penetration test or the North American performance specification, which requires no visible fog after the fogging test and sets dew point criteria (ASTM International, 2019b). In buildings with high indoor humidity, tell the glass manufacturer about it so that desiccant quantity and seal specification can be matched.
Hypothesis 4: migration from glazing
Glazing sealants, setting blocks, gaskets, backing and repair sealant applied on site all touch the unit's edge, so their ingredients can become the problem. It applies especially when products high in solvents or plasticisers are used, when the glass manufacturer has not confirmed a product, or when a different sealant has been applied over the original during repairs. Say a window had its perimeter sealant repaired with a different sealant over the original. About a year later, an oily-looking smear appears along the inner edge of the glass, and inside it a hazy film spreads that does not clear whatever the weather.
The trouble is that materials in contact exchange ingredients. The potentially incompatible substances from glazing components include organic ones such as plasticisers, volatile vapours, oils and solvents, and they can spread not only between materials in contact but throughout the glazing system. The result can be primary seal or incompatible material migrating beyond the sealant sightline, loss of adhesion, weaker moisture and gas retention, and poor appearance (FGIA & NGA, 2023). Early glazing design guidance already warned that solvents in one material may harm another (Garden, 1964). Organic vapours that reach the space between the panes react with glass surfaces dampened by water vapour and leave a permanent opaque deposit, which is called chemical fogging (Van Den Bergh et al., 2013).
Listing the materials that touch the glass edge comes first. Gather product names and installation dates of glazing sealants, setting blocks, gaskets, backing and any repair sealant, and see whether fogged units appear together with a particular material or repair period. Check whether the dark primary seal line has crept into the glass area and whether there is an oily smear at the edge. Compatibility between materials is confirmed by a test that measures how a glazing material affects the adhesion and cohesion of the unit's edge sealant, and by a test that exposes accessories and sealant together to heat and ultraviolet light and then checks colour and adhesion (ASTM International, 2020a, 2023).
Let only materials with confirmed compatibility touch the edge. Specify glazing sealants, setting blocks and gaskets as combinations whose compatibility both the glass manufacturer and the sealant supplier have confirmed, and use the original or confirmed materials for repairs too. The test for liquid-applied glazing materials only looks at the effect on the unit's edge sealant and does not address hermetic seal integrity or changes in the vision area, so to cover the primary seal, ask separately for a compatibility test against the butyl primary seal (ASTM International, 2020a). A North American industry document has validated a German institute's test method for this purpose and recommends it (FGIA & NGA, 2023).
Hypothesis 5: water in the rebate
When fog starts at the bottom edge of the units and the drainage at the bottom of the frame is in doubt, standing water is the first suspect. This covers windows with no drainage holes or with holes blocked by dirt, insects or sealant applied over them, windows where the bottom edge of the unit rests directly on the frame with no setting blocks, and windows where rain easily gets in past the glazing beads. Picture a window whose bottom rail drainage holes are blocked by dirt and sealant applied over them. With one glazing bead removed after rain, the bottom edge of the unit is standing in water, and the fog is densest near that edge.
Water attacks the edge seal from two directions. Organic secondary sealants left in contact with water for long periods absorb a great deal of it and swell considerably, and the swelling opens the primary seal so that more water vapour gets in. Water can also hydrolyse chemical bonds at the glass surface and irreversibly damage the sealant's adhesion to glass, which is why glazing guidelines attach great importance to keeping the rebate free of water (Wolf, 2002). The butyl primary seal's adhesion does not withstand continuous water either; once damp, it loses its grip and the unit can fail early (Van Den Bergh et al., 2013). It was pointed out long ago that the glazing space should always drain to the outside, because water can enter from rain or condensation, and that standing water speeds the deterioration of glazing materials (Garden, 1964).
Remove one bottom glazing bead and look. Check for water or tide marks at the bottom of the rebate, whether the setting blocks are in place supporting the bottom edge, and whether the secondary sealant is wet, swollen or lifting. Check the drainage holes for blockage from outside, and pour a little water into the rebate to see whether it drains within a set time. Placing a small data logger in a suspect window is another option, following the example of a study that measured temperature, relative humidity and the presence of liquid water around the edge seal inside window frames over several years (Garvin & Wilson, 1998).
Restore drainage first, then replace the glass. Clear blocked drainage holes or make new ones, lift the bottom edge of the unit off the rebate floor with setting blocks, and remove any repair sealant covering the drainage holes. Replacing only the fogged units while leaving a frame that holds water sends the new units the same way, so check drainage on the other windows of the same elevation too. Add cleaning of drainage holes to routine inspections.
Finding the cause
First confirm that the fog really is between the panes. Condensation on the room-side or outside face is a matter of indoor humidity or the glass's insulation, not of the seal, so start by wiping both faces. After that, look at what can be seen without opening anything: the position and orientation of fogged units, drainage holes, edge exposure and the materials in contact. Dew point measurement and cutting units open come after that.
The distribution of fogged units narrows the cause. Fog starting at the bottom edge and clustered in windows with blocked drainage points to standing water, and fog clustered in sloped or tinted glass with sun-exposed edges points to secondary sealant ageing. If only a few new units from the same lot fogged early, suspect the primary seal; if units of the same age fog one after another evenly across the building, suspect saturated desiccant; and if fog appeared with an oily smear after repairs or after a particular glazing material was used, suspect migrating ingredients.
The nature of the fog is also a clue. Chemical fogging left by organic vapours remains as a permanent deposit (Van Den Bergh et al., 2013). Fog from water vapour, by contrast, thickens and thins over and over with glass temperature. A white film that does not clear when the weather warms puts migrating ingredients on the list as well. There is also a standard test for resistance to fogging by volatile components, and its results can be requested when choosing new units (ASTM International, 2019a).
If that still does not settle it, remove one fogged and one clear unit from the same position and compare them. Measure the dew point of both, then cut the edges and look in turn at the continuity and width of the primary seal, the adhesion of the secondary sealant and the moisture content of the desiccant. Put a new unit in the opening after correcting drainage and setting blocks, and measure its dew point over several seasons alongside neighbouring windows in the same conditions. If the new unit's dew point stays close to its starting value, the cause has been put right.
The hypotheses can overlap. A secondary sealant standing in water swells and opens the primary seal, and the moisture that gets in that way fills the desiccant sooner than planned. In sloped glazing, water, heat and sunlight attack the edge all at once. In such cases, put right the conditions that can be changed in the frame and on site, such as drainage and edge protection, and then look at the units and materials, because in a frame that holds water and lets sun onto the edge, no unit can be compared fairly.
Limits and cautions
Primary seal dimensions, secondary sealant type, desiccant quantity and acceptable glazing materials differ by glass manufacturer and product, so decisions follow the manufacturer's glazing instructions and product data. Drilling and drying fogged units on site does not restore the seal and may void the warranty, so consult the manufacturer first. Replacing structurally glazed curtain wall units and safety glass is work for the designer and a specialist installer.
Safety matters too. Insulating glass units are heavy and their edges sharp, so use equipment such as suction lifters and cut-resistant gloves when removing and carrying them, with at least two people handling each unit. Work on upper-floor glass from a lift or gondola with fall protection. For sealants, primers and cleaning solvents, follow the product's safety data sheet, the SDS, for ventilation and protective equipment.
Sources
- ASTM International. (2019a). ASTM E2189-19, Standard test method for testing resistance to fogging in insulating glass units. https://store.astm.org/e2189-19.html
- ASTM International. (2019b). ASTM E2190-19, Standard specification for insulating glass unit performance and evaluation. https://store.astm.org/e2190-19.html
- ASTM International. (2020a). ASTM C1294-20, Standard test method for compatibility of insulating glass edge sealants with liquid-applied glazing materials. https://store.astm.org/c1294-20.html
- ASTM International. (2020b). ASTM E546-14(2020), Standard test method for frost/dew point of sealed insulating glass units. https://store.astm.org/e0546-14r20.html
- ASTM International. (2023). ASTM C1087-23, Standard test method for determining compatibility of liquid-applied sealants with accessories used in structural glazing systems. https://store.astm.org/c1087-23.html
- European Committee for Standardization [CEN]. (2018). EN 1279-2:2018, Glass in building — Insulating glass units — Part 2: Long term test method and requirements for moisture penetration.
- Fenestration and Glazing Industry Alliance [FGIA], & National Glass Association [NGA]. (2023). Compatibility testing of insulating glass PIB primary sealant with respect to glazing materials (IGMA TB-1300-23 / NGA FB75-23). https://www.glass.org/sites/default/files/2023-06/NGA-FB75-23_IGMA-TB-1300-23_Compatibility_Testing_PIB_final.pdf
- Garden, G. K. (1964). Glazing design (Canadian Building Digest CBD-55). National Research Council of Canada. https://web.mit.edu/parmstr/Public/NRCan/CanBldgDigests/cbd055_e.html
- Garvin, S. L., & Wilson, J. (1998). Environmental conditions in window frames with double-glazing units. Construction and Building Materials, 12(5), 289–302. https://doi.org/10.1016/S0950-0618(98)00008-7
- Van Den Bergh, S., Hart, R., Jelle, B. P., & Gustavsen, A. (2013). Window spacers and edge seals in insulating glass units: A state-of-the-art review and future perspectives. Energy and Buildings, 58, 263–280. https://doi.org/10.1016/j.enbuild.2012.10.006
- Wolf, A. T. (1992). Studies into the life-expectancy of insulating glass units. Building and Environment, 27(3), 305–319. https://doi.org/10.1016/0360-1323(92)90032-K
- Wolf, A. T. (2002). Design and material selection factors that influence the service-life and utility value of dual-sealed insulating glass units. In Proceedings of the 9th International Conference on Durability of Building Materials and Components (Paper 106). Brisbane. https://www.irbnet.de/daten/iconda/CIB9944.pdf