Watching the trend until it nears the alarm, or simply changing the oil, is the usual response to a journal bearing that creeps hotter, but temperature signals that the balance between heat made in the oil film and heat carried away by the oil has shifted, so unless the cause of that shift is found, it tends to climb again on fresh oil. What actually drives it up can be oil supply cut by blocked orifices and filters, a fouled oil cooler, the wrong viscosity grade, oxidised oil, a bearing surface damaged by debris or a shift in shaft alignment, and sometimes two or more at once.
Background
Overlay a few months of bearing temperature trends from a compressor, pump or turbine, and the line tilts gently upwards. Day to day the change is small and easy to pass over, but as the margin to the alarm shrinks, one hot day or one heavy-load day can bring an alarm or a trip. When a journal bearing runs hot, babbitt, the soft alloy lining the bearing surface, softens, and if the oil film breaks the shaft and bearing touch directly and can seize. At that point it means not just a new bearing but shaft repair and a long outage.
An oil-fed journal bearing carries its load by hydrodynamic lubrication: oil dragged in by the turning shaft builds pressure in a wedge-shaped gap and lifts the shaft. The work spent shearing the film turns into heat, and most of that heat is carried off by the oil leaving the bearing. Bearing temperature is therefore set by the balance between heat made in the film and heat carried away by the oil, and that balance depends on oil viscosity, supply temperature and flow, and the shape of the gap between shaft and bearing (Khonsari & Booser, 2017).
A slow rise means one side of this balance is moving slowly. The oil carrying heat away may have dropped in flow or got hotter, the heat made by the film may have grown, or the gap may have changed shape so that the film is thinner on one side. Even for the same rise, whether it crept up evenly over months or jumped a step after maintenance or a top-up separates the causes sharply.
In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: lay the bearing temperature trend on the same time axis as supply pressure, oil temperatures before and after the cooler, load and vibration, mark the dates of maintenance and top-ups, and compare them with the lubricant's technical data sheet, the TDS, and the equipment design conditions.
Hypothesis 1: reduced oil supply
Oil runs from the pump through the filter to the header, and an orifice, a small restriction ahead of each bearing, divides the flow. Less oil reaches the bearing when contaminants load the filter and raise its pressure drop, when sludge or debris narrows an orifice or feed hole, or when the pump wears or the pressure regulating valve drifts. Picture the lube system of a fan. The header pressure gauge has crept down over the months almost unnoticed, the filter differential gauge has risen close to its change mark, and the stream of oil visible through the bearing drain sight glass is thinner than before.
With less flow, less oil has to carry the same heat, so the oil warms more as it passes the bearing and the bearing metal temperature follows. In experiments and analysis on a single-groove journal bearing, every supply condition studied, supply pressure and temperature among them, changed the flow markedly (Costa et al., 2003). In a model of tilting-pad bearings running short of oil, once flow fell below a certain level, starved regions appeared first on unloaded pads, and with further cuts spread to the loaded pads, changing film temperature and even the dynamic behaviour (San Andrés et al., 2018). So when flow falls, temperature may at first rise only a little and then climb quickly once starvation reaches the loaded surface.
Measure both header pressure and the pressure just ahead of the bearing to see where pressure is lost. Check in turn the filter differential pressure record, pump discharge pressure and the regulating valve setting, and compare the temperature rise from oil in to oil out at each bearing. A bearing whose rise is markedly larger than the others may be short of flow, so at the next stop pull its orifice and feed holes and look for blockage.
Once reduced supply is shown to be the cause, change the filter, clean blocked orifices and feed holes, and measure again to confirm design flow and pressure have returned. Note what blocked the orifice as well: sticky deposits call for a look at oil oxidation too, and metal or sand-like grains at debris. Set a rule to change filters before the differential pressure reaches a set value.
Hypothesis 2: fouled oil cooler
If bearing temperature rises every summer and the rise grows year by year, suspect the oil cooler. The cooler cannot cool the oil enough when scale, biofilm or silt builds on the water side, sludge coats the tubes on the oil side, the cooling water valve is not fully open, or the temperature control valve is not doing its job. Think of a pump whose cooling water inlet temperature is much the same as this time last year, yet whose cooler outlet oil temperature is logged higher. Supply pressure and load are unchanged.
A fouling layer on a heat exchanger surface acts as insulation in its own right and cuts the heat that can be moved into the same cooling water (Bott, 1995). When the cooler does less, oil enters the bearing hotter, so bearing temperature starts from a higher base. Hotter oil also has a lower viscosity, which thins the film. In a study of single-groove journal bearings, it was supply temperature, more than supply pressure or groove geometry, that mainly governed power loss, maximum bearing temperature and minimum film thickness (Costa et al., 2003). That is why a loss of cooler performance shows up directly in bearing temperature.
Judge cooler performance from four temperatures. Measure oil inlet and outlet and cooling water inlet and outlet together, and compare them, with cooling water flow and the pressure drop on each side, against design values or records from when the cooler was clean. If water inlet temperature is unchanged but the gap between oil outlet and water outlet temperatures has widened, less heat is crossing inside the cooler. If there is a temperature control valve, confirm it actually opens and closes.
Switch to the standby cooler and clean the fouled one. Remove water-side scale and biofilm by chemical or mechanical cleaning, and review the cooling water treatment so it does not build up again. If sludge coats the oil side, cleaning the cooler alone is not enough, so check the oil condition as well. After cleaning, measure the four temperatures again and keep them as a baseline, so the next fouling is caught early.
Hypothesis 3: wrong viscosity grade
If bearing temperature shifted a step after a top-up or oil change, look at viscosity first. Typical cases are cutting the number of lubricants and merging similar grades, topping up in a hurry with another grade from the store, and changing supplier. Suppose that at a routine top-up the usual grade had run out, and the oil one grade heavier meant for the next machine went in. From that week the bearing temperature trend runs flat a few degrees higher, and with the seasonal swing laid on top, it looks like a slow rise.
Viscosity sets both the heat made in the film and the film thickness. Higher viscosity thickens the film but raises the work of shearing it, so more heat is made; lower viscosity makes less heat but thins the film and cuts the margin at high load or low speed (Khonsari & Booser, 2017). Industrial lubricant viscosity grades are defined by the midpoint kinematic viscosity at 40 °C, with 10% either side of that value allowed for each grade (ISO, 1992). One grade's difference lies well outside that band, so an oil other than the design grade sets a new heat balance for the bearing.
Confirm it from both records and a sample. Check the names and grades of the last few top-ups in the records, and measure the kinematic viscosity at 40 °C of a sample of the oil in service by the standard method (ASTM International, 2024) to see whether it falls within the design grade's range. See also whether the step in the temperature trend lines up with a top-up date.
If viscosity is out of range, return to the design grade. When a large share has been mixed, a partial change rarely corrects it, so change the oil following the equipment maker's procedure. Mark top-up containers and fill points with the same grade label, and before merging products or changing supplier, confirm with the supplier that viscosity grade and performance specification match.
Hypothesis 4: oxidised oil
This hypothesis comes forward in equipment where the oil has been in service a long time, where it often passes hot spots, or where a large reservoir gets so little make-up that almost no fresh oil goes in. Here bearing temperature rises over months to years, sometimes with vibration rising alongside. A turbine lube system is opened at a stop to change filters: the pleats carry a brown film, the tank walls show glossy, varnish-like stains, and the oil is clearly darker than when new.
Oxidation is the slow breakdown of oil as it meets heat and oxygen from the air. As it proceeds, acids form, viscosity rises and oxidation products that do not dissolve in the oil build up. A study of turbine bearing pads reported that under severe conditions deposits form on the loaded part of the pad, and that excessive build-up can raise temperature and vibration to unacceptable levels. The deposits were mainly organic compounds produced as oxidation by-products, and insoluble oxidation products in the oil acted as their precursor (Yokoyama et al., 2015). Deposits change the shape of the bearing gap and block the path by which heat leaves through the metal, while oil whose viscosity has risen makes more heat in the film.
Oil analysis separates oxidation out. The standard practice for monitoring turbine oils in service sets tests such as viscosity, acid number and oxidation stability at fixed intervals and advises interpreting the values according to the equipment and its operation (ASTM International, 2022). Compare against new oil and earlier results to see whether viscosity and acid number are climbing, and check insoluble oxidation products by membrane patch colorimetry, which filters the oil through a membrane and measures the colour left on it (ASTM International, 2021). At a stop, look directly for brown or black films on the bearing pads and orifices.
Once oxidation is confirmed, changing the oil alone falls short. Deposits left in the system can be taken up by the new oil and laid down again, so agree a flushing method and deposit-removal filtration with the oil supplier before the change. Fix the hot spots that sped oxidation as well, such as a fouled cooler or an excessive supply temperature. After the change, run the same tests at the same intervals so the new oil's trend is recorded from the start.
Hypothesis 5: debris-scored surface
If temperature began to rise after an overhaul or pipework and solid particles in the oil have increased, debris may have damaged the bearing surface. It happens when flushing after maintenance fell short, when dust gets in through tank breathers or shaft seals, when another part wears and sheds metal fines, or when the filter has run with its bypass valve open. Take a machine restarted after gearbox work: bearing temperature holds for the first few days, then creeps up over several weeks, and fine grains settle at the bottom of the oil sample bottle.
The babbitt lining a journal bearing is soft enough to bury small particles in its surface, but that ability has limits. The damage contaminant particles do to a bearing depends on their size and hardness and on how they compare with the film thickness, and particles embedded in the bearing face can create momentary high temperatures at the sliding contact that lead to scuffing (Khonsari & Booser, 2006). Score lines and embedded particles roughen the bearing surface and eat into the margin where the film is thinnest. If the shaft is scored as well, the same thing tends to repeat in a new bearing.
The amount of particulate can be put into numbers with an oil cleanliness count. Use the method that counts particles by size and expresses them as a code (ISO, 2021), and compare values before and after maintenance and with other bearing systems. Check the filter differential pressure record for signs that the bypass opened, and whether the tank breathers are filtered. If the bearing can be opened at a stop, look for score lines and embedded grains in the babbitt and scoring on the shaft, and magnify the filtered grains to tell metal fines from sand and trace their source.
If debris is the cause, the first step is to filter the oil back within the equipment's cleanliness target, and after an overhaul to flush the whole system. Fit breathers with particle and moisture protection, and change filters before the bypass opens. If the bearing face or shaft is already damaged, the bearing may need replacing or the shaft dressing depending on the extent, a call to make together with a bearing repair specialist.
Hypothesis 6: shaft misalignment
If oil and cooling are fine but only one bearing runs hotter, and only the temperature sensor near one end of it, look at alignment. Typical cases are a settling foundation or twisted baseplate, pipework pulling on the machine, thermal growth at running temperature that differs from what was allowed for when aligning, and the period after a coupling or motor change. An example is a compressor realigned after a motor change, where a few weeks later only the bearing nearest the motor runs hotter than the others, and shaft vibration at the same spot slowly grows with it.
When the shaft tilts inside the bearing, the gap becomes uneven along the axis, so the film thins at one end and pressure and heat concentrate there. A study that combined analysis and experiment on misaligned journal bearings concluded that misalignment raises bearing temperature and markedly reduces the minimum film thickness (Pierre et al., 2004). In tests on a 100 mm diameter journal bearing under a misaligning torque, performance changed more at low speed or low load (Bouyer & Fillon, 2002). A film that generates less force can be read as resisting the tilt less.
The clue lies in temperature differences within the same bearing. If there are sensors at both ends or several positions, see whether the gap between them is widening, and whether that bearing's vibration trend has changed along with its temperature. At a stop, measure cold alignment with a laser alignment tool, and if possible measure at running temperature as well to capture thermal growth. When a bearing is next opened after maintenance, look for a contact mark on the babbitt skewed towards one end.
If alignment has shifted, realign to targets that allow for thermal growth at running temperature. Unless the causes that will throw it out again are fixed too, such as soft foot, where a foot does not sit evenly on its base, pipe loads pulling on the machine and foundation settlement, the same rise will be back within months. After realigning, keep the end-to-end temperature difference and vibration of that bearing as a baseline.
Finding the cause
The six hypotheses need not be searched all at once. Rule them out starting with what instruments and records show while running. Supply pressure, filter differential pressure and the four cooler temperatures can be read today, and viscosity, oxidation and cleanliness can all come from one bottle of oil sample. Opening the bearing and measuring alignment need a stop, so they come last.
The shape of the rise narrows the field. An even rise over months shared by several bearings points to what they all share: oil supply, the cooler and oil oxidation. Among those, look at the cooler if supply temperature has risen too, at filters and orifices if supply temperature holds but pressure has dropped, and at oxidation if both hold but the oil analysis is worsening. A step that lines up with a top-up or maintenance date points to whatever changed then, such as viscosity grade, debris or alignment.
If only one bearing is rising, the cause lies with that bearing rather than the whole system. If the oil temperature rise across that bearing alone is large, look first at its orifice; if only one end of the bearing is hot, at alignment; and if particles come mainly from that bearing's drain, at debris damage.
Settle remaining doubt by changing one thing at a time. Fitting a new filter, switching to the standby cooler and returning the oil to the design grade must each be done separately, or there is no seeing which one worked. Afterwards, compare bearing temperature at the same load and cooling water temperature with the values before the change, and count the job done when the trend line has returned to its earlier slope.
The hypotheses can also interlock. A fouled cooler raises supply temperature and speeds oil oxidation, and the deposits from oxidation in turn block orifices and the oil side of the cooler. A surface scored by debris has less film margin, so small errors in alignment or viscosity swing the temperature further. When they appear together, first put right what carries heat away, the oil supply and the cooler, then bring the oil condition back, and only then look at the bearing and alignment. While supply and cooling are unsettled, the effect of other measures cannot be compared fairly.
Limits and cautions
Bearing temperature alarm and trip values, supply pressure and flow, oil grade and analysis limits, and alignment tolerances differ by equipment and bearing design, so numeric decisions follow the equipment maker's guidance and the oil's TDS. If temperature climbs quickly or vibration rises sharply with it, that is a time to reduce load or stop under the operating procedure rather than watch the trend, and judging and rebuilding a damaged bearing is work for a bearing repair specialist.
Safety matters too. Oil in a running lubrication system is hot and under pressure, so isolate the system and release pressure before opening a filter or orifice. Before opening a bearing or measuring alignment, isolate the machine's energy sources and apply locks and tags (OSHA, n.d.). Handle oils and cleaning agents with gloves and eye protection as the safety data sheet, the SDS, directs.
Sources
- ASTM International. (2021). ASTM D7843-21, Standard test method for measurement of lubricant generated insoluble color bodies in in-service turbine oils using membrane patch colorimetry. https://store.astm.org/d7843-21.html
- ASTM International. (2022). ASTM D4378-22, Standard practice for in-service monitoring of mineral turbine oils for steam, gas, and combined cycle turbines. https://store.astm.org/d4378-22.html
- ASTM International. (2024). ASTM D445-24, Standard test method for kinematic viscosity of transparent and opaque liquids (and calculation of dynamic viscosity). https://store.astm.org/d0445-24.html
- Bott, T. R. (1995). Fouling of heat exchangers. Elsevier.
- Bouyer, J., & Fillon, M. (2002). An experimental analysis of misalignment effects on hydrodynamic plain journal bearing performances. Journal of Tribology, 124(2), 313–319. https://doi.org/10.1115/1.1402180
- Costa, L., Miranda, A. S., Fillon, M., & Claro, J. C. P. (2003). An analysis of the influence of oil supply conditions on the thermohydrodynamic performance of a single-groove journal bearing. Proceedings of the Institution of Mechanical Engineers, Part J: Journal of Engineering Tribology, 217(2), 133–144. https://doi.org/10.1243/13506500360603561
- International Organization for Standardization [ISO]. (1992). ISO 3448:1992, Industrial liquid lubricants: ISO viscosity classification.
- International Organization for Standardization [ISO]. (2021). ISO 4406:2021, Hydraulic fluid power: Fluids: Method for coding the level of contamination by solid particles. https://www.iso.org/standard/79716.html
- Khonsari, M. M., & Booser, E. R. (2006). Effect of contamination on the performance of hydrodynamic bearings. Proceedings of the Institution of Mechanical Engineers, Part J: Journal of Engineering Tribology, 220(5), 419–428. https://doi.org/10.1243/13506501J00705
- Khonsari, M. M., & Booser, E. R. (2017). Applied tribology: Bearing design and lubrication (3rd ed.). Wiley.
- Occupational Safety and Health Administration [OSHA]. (n.d.). Control of hazardous energy (lockout/tagout). U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/control-hazardous-energy
- Pierre, I., Bouyer, J., & Fillon, M. (2004). Thermohydrodynamic behavior of misaligned plain journal bearings: Theoretical and experimental approaches. Tribology Transactions, 47(4), 594–604. https://doi.org/10.1080/05698190490513974
- San Andrés, L., Koo, B., & Hemmi, M. (2018). A flow starvation model for tilting pad journal bearings and evaluation of frequency response functions: A contribution toward understanding the onset of low frequency shaft motions. Journal of Engineering for Gas Turbines and Power, 140(5), 052506. https://doi.org/10.1115/1.4038043
- Yokoyama, F., Iwama, Y., Maruyama, M., & Sano, M. (2015). Deposits on bearing pad caused by particulate contamination in turbine oil. Tribology Online, 10(2), 162–171. https://doi.org/10.2474/trol.10.162