KALTECKOREA

BlogApplication notes

Why does lapping leave deep scratches?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Switching to a finer abrasive or lapping for longer is the usual response to deep scratches on a lapped face, but scratches are left by the few particles that carry the load on their own, not by the average grain, so unless their source is found they come back. What actually lies behind them can be oversized particles that got in, an unstable slurry that clumps or settles, lean slurry, dirty carriers and plate, or a damaged plate surface, and sometimes two or more at once.

Background

Mechanical seal faces, valve plates or ceramic parts come off the lap, and turned under the light, an even matt surface carries one or two unusually deep scratches. Flatness and thickness are in tolerance, yet that one scratch makes the part a reject. Within a single batch, some parts come out clean while others alone carry scratches.

Lapping is often the final precision step, so a scratched part carries the whole cost of the steps before it. Deep scratches do not polish out easily, so the part is lapped again from the start or, with its thickness allowance gone, scrapped. On a seal face a scratch can become a leak path, and on an optical part or substrate it is a quality defect in itself.

Lapping feeds a slurry of abrasive between a plate and the workpiece, and the loose particles between them carry the load and remove material little by little (Klocke, 2009). Particles move between rolling, which leaves small indents, and being embedded in or held by one face and sliding, which cuts grooves, and the look of the lapped surface depends on which dominates (Evans et al., 2003). A deep scratch can be read as the track of a particle dragged under an unusually large share of the load, so finding the cause means asking where that particle came from and why it was dragged.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: record each scratch's length, direction and width, with the part, carrier position and place in the batch where it appeared, and compare the grit, concentration, feed rate and agitation of the slurry used at the time with the slurry's technical data sheet, the TDS, and the process settings.

Hypothesis 1: oversized particles

Oversized particles get in by many routes: a new abrasive lot, coarse and fine stages run alternately on one machine, dried slurry crust breaking off nozzles and tank walls, dust from a grinding area settling into an uncovered tank, and chipping at the edges of brittle workpieces. Say scratches start on the day slurry is made from a freshly opened abrasive drum, while batches run on slurry left from the previous lot stay clean; then this hypothesis comes first.

Scratches are made not by particles of average size but by the few large ones at the tail of the distribution. A large particle catches between the two faces before its neighbours, carries the load alone, and is dragged instead of rolling, cutting a groove. In one study, spiking a chemical mechanical polishing slurry with coarser silica at the level of the detection limit caused surface damage and changed the removal rate (Basim et al., 2000). In another, the count of large particles in the slurry and the count of scratches on the surface followed a straight-line relationship (Remsen et al., 2006). Abrasive grit is defined by a distribution, not a single average, so the standard also sets out how to determine and designate the distribution of microgrits (ISO, 2007).

Measure the particle size distribution of fresh and used slurry by laser diffraction and compare them with each other and with the TDS (ISO, 2020). A very small number of large particles is easily lost within the overall distribution, though, so methods that count large particles one by one, like those in the study above, are used separately. On the floor, simply passing slurry through a fine sieve or filter paper and looking at what is left under a microscope gives clues. Fragments that are not abrasive in shape, or chips from the workpiece, hint at how they got in.

Once oversized particles are confirmed, cut off their route in. Give each grit its own machine, tank and tools, or where that is not possible, set a full wash-down sequence for grit changes. Cover tanks, and scrape off dried crust before it can fall. Accept a new abrasive lot only after measuring its distribution, and pass slurry through a set mesh before it is fed.

Hypothesis 2: unstable slurry

Suspect it where slurry stands overnight without agitation, where feed lines are long or have stretches where flow stops, and where the pH of water-based slurry is not controlled. Scratches sometimes cluster in the first batch of the morning and fall away after one or two batches. Prod the bottom of the mixing tank with a rod and a hard layer is there, and when the stirrer starts again in the morning, that layer breaks away and floats about in lumps.

Gravitational settling speeds up with the square of particle size (ISO, 2001), so when agitation stops, the largest particles gather on the bottom first. If they do not disperse evenly when stirred again, large particles and lumps go out together in the first part of the feed. A clump of particles stuck together carries load between plate and workpiece like a single large particle. A study of silicon carbide slurry for sapphire lapping reported that particle agglomeration varies with slurry pH and that matching grit and pH can reduce scratches (Yin et al., 2021). A basic rule of slurry design is that the abrasive must stay stably dispersed even under the dynamic conditions of processing if polishing is to be low in defects (Basim & Moudgil, 2003).

Stand slurry in a graduated cylinder and compare the time for the top to clear and the depth of the bottom layer with fresh slurry. If the bottom layer, rubbed between the fingers, is packed hard and does not break up again, it is caked sediment. For water-based slurry, measure pH against the TDS range, and look at slurry caught at the feed nozzle under a microscope for lumps. Check the records, too, for scratches clustering just after agitation restarts or feed begins.

For an unstable slurry, constant agitation and circulation come first. Keep the tank stirred without pause, shorten the lines so no stretch has standing flow, and circulate slowly even during breaks. Remove caked sediment rather than breaking it up for reuse, and keep pH and dispersant for water-based slurry within the supplier's recommended range. Before the first batch of the morning, circulate thoroughly before feeding begins.

Hypothesis 3: lean slurry

Concentration drops when feed is cut back to save abrasive, when a feed nozzle is half blocked, and when topping up adds only carrier fluid. A wide plate with feed falling in one spot only, so part of the plate runs starved, has the same effect. Suppose that after the feed pump is turned down a step to save abrasive, the drops come further apart and the outer band of the plate starts running shiny and dry. Scratches turn up mainly on parts in the outer carriers.

Whether particles roll or are dragged depends on the balance between load and the number of particles. In micro-scale abrasion tests, the boundary between rolling wear and grooving wear was set by the ratio of load to slurry concentration, with higher load and lower concentration pushing towards grooving (Trezona et al., 1999). When slurry thins, fewer particles share the same load, so each one is pressed harder and more easily embedded or dragged. In sapphire lapping tests, raising slurry concentration also raised the removal rate (Yin et al., 2021), so a lean slurry can add scratches while also slowing removal.

The check is made on the feed side. Catch slurry at the nozzle for a set time to measure feed rate, dry a set volume of it and weigh the solids to find concentration, and compare with the TDS. Watch the turning plate to see whether the slurry film wets it evenly or leaves a dry band. If scratches cluster at a particular plate radius or in carriers far from the feed point, feed is uneven.

For a lean slurry, start by bringing feed rate and concentration back within the TDS range, and top up with slurry at the set concentration rather than fluid alone. On wide plates, add or move feed points so the whole plate is wetted evenly. At the start of a run, raise pressure only after the slurry has spread across the plate, and add blockage-prone nozzles to the check list.

Hypothesis 4: dirty carrier and plate

The settings for this hypothesis are the step from coarse to fine grit, shops where carriers are shared across machines or grits, carriers whose worn edges are crumbling, and plates whose grooves hold old, hardened slurry. Consider a plate given a single wipe with a cloth after coarse lapping, with finish lapping then started using the same carriers. Deep scratches appear only in the first finishing batch, and their width resembles the marks of the previous stage's abrasive.

Coarse particles left in a fine stage do the same as oversized particles mixed in. As noted above, scratch counts rise along with the count of large particles in the slurry (Remsen et al., 2006). Coarse grains stay where a cloth does not reach, such as the edges of carrier pockets, the seats where parts sit and the bottoms of plate grooves, and come loose into the slurry again during finish lapping. Fragments from worn carrier edges and chips broken from workpieces take the same path. So changing the slurry at each stage, without cleaning carriers and plate to the same standard, changes only the slurry.

Take the carriers out and look at them under a magnifier. Search for particles embedded at pocket edges and floors, worn and lifting edges and cracks, and scrape the bottoms of plate grooves to see whether old slurry comes out. If scratches cluster in the batches right after a grit change and fade a few batches later, contamination is the cause. Use the records, too, to see whether scratches come only from particular carrier numbers.

If contamination is the cause, keep separate carriers for each grit, and at grit changes clean carriers ultrasonically and brush plates out down into the grooves. Set a replacement rule for carriers with worn or cracked edges, and wash previous-stage slurry off workpieces before they go into the next stage. Splitting coarse and finishing stages into separate rooms or areas also cuts airborne particles.

Hypothesis 5: damaged plate

Look at this hypothesis with plates left long without reconditioning, plates whose grooves have worn shallow, plates nicked and burred by dropped tools or parts, and soft plates in use with large particles embedded. On a plate run for months without reconditioning, the once-sharp groove edges may have worn round, and a straightedge may show the height varying along the radius. Parts from that plate show scratches and, alongside them, slowly worsening flatness.

The plate surface decides how slurry stays under the workpiece. In a sapphire lapping study, a low groove density, the ratio of groove width to groove pitch, let the fluid film thicken until the workpiece hydroplaned on it, and once the film was thicker than the abrasive, only the large particles took part, raising roughness and worsening flatness (Lee et al., 2020). Something similar can happen on a plate whose grooves have worn shallow. Because of the geometry of lapping motion, a plate does not wear evenly along its radius, and motion settings, such as the position of the conditioning rings, can be chosen to correct its flatness error (Barylski & Piotrowski, 2018). Coarse particles embedded in the plate, or raised burrs, act like fixed abrasive, dragging across the workpiece and cutting grooves (Evans et al., 2003).

Start by running a hand over the plate and looking closely. Feel for nicks and burrs that catch the fingertip, look for embedded particles showing as bright points, and compare groove depth and edges with the drawing of a new plate. Measure flatness along the radius with a straightedge and feeler gauge or a dial gauge, and log the trend since the last reconditioning. If scratches recur at the same place on the workpiece or grow along with worsening flatness, the plate is the cause.

Resurface a damaged plate before further use. Remove nicks and burrs, correct flatness by moving the conditioning rings or refacing the plate, and recut worn grooves. Set the reconditioning interval by measured flatness and groove depth rather than by the calendar, and make it a rule that no tools or parts are set down on the plate.

Finding the cause

Do not search all five at once. Rule out first what hands, eyes and simple tools can check in minutes. The shape and position of scratches, slurry feed and how the plate is wetted, sediment in the tank, and the condition of carriers and plate can be seen right beside the line. Slower work, such as particle size analysis and plate flatness measurement, comes after.

The first clue is when scratches appear. If they cluster right after a new abrasive lot or a grit change, look at oversized particles that got in and coarse particles left behind; if they cluster in the first batch of the morning or right after agitation restarts, look at settled or clumped slurry. If they grow slowly over time along with worsening flatness, suspect a damaged plate surface.

Next is position. Scratches on particular carrier numbers point to contamination and wear on those carriers; scratches clustered at one plate radius or far from the feed point point to uneven feed and lean slurry; and scratches recurring at the same place on the workpiece point to a nick or embedded particle in the plate. Scratches scattered at random through the batch point to oversized particles spread through the whole slurry.

If that still does not settle it, run control trials that change one thing at a time. Run new-lot slurry both filtered and unfiltered, load clean new carriers and used ones in the same batch, and compare a reconditioned plate with the one in use. Change only one thing at a time, or there is no telling what worked. Afterwards, inspect a set number of parts under fixed lighting and magnification and count the share with scratches on the same basis as before, and the job is done only when that figure has come down.

The hypotheses overlap. In a lean slurry even a few large particles take a bigger share of the load, shallow worn grooves hold old slurry and coarse grains and so add to contamination, and lumps broken from caked sediment cannot be told apart from oversized particles. In such cases put cleanliness right first, filtering slurry and washing carriers and plate, then concentration and agitation, and the plate surface last, because in a dirty system the effect of changing concentration or the plate cannot be compared fairly.

Limits and cautions

Suitable grit, slurry concentration and feed rate, pressure and plate reconditioning interval differ by workpiece material, plate material, abrasive type and required quality, so numeric decisions follow the slurry's TDS and the equipment and plate suppliers' guidance. Scratch judgement changes with lighting, magnification and viewing angle, so first make sure supplier and customer inspect under the same conditions. For functional surfaces such as seal faces, optical parts and semiconductor substrates, do not release on floor judgement alone; get the quality engineer to confirm.

Safety matters too. Wear gloves and eye protection for slurries and cleaners as the product's safety data sheet, the SDS, directs, and keep abrasive wet so dry powder does not become airborne. Spent slurry and residue from plate reconditioning contain workpiece material, so dispose of them under local waste rules. Run a hand over the plate only after the machine is fully stopped and locked out.

Sources

  1. Barylski, A., & Piotrowski, N. (2018). Non-conventional approach in single-sided lapping process: Kinematic analysis and parameters optimization. The International Journal of Advanced Manufacturing Technology, 100(1–4), 589–598. https://doi.org/10.1007/s00170-018-2644-z
  2. Basim, G. B., & Moudgil, B. M. (2003). Slurry design for chemical mechanical polishing. KONA Powder and Particle Journal, 21, 178–184. https://doi.org/10.14356/kona.2003020
  3. Basim, G. B., Adler, J. J., Mahajan, U., Singh, R. K., & Moudgil, B. M. (2000). Effect of particle size of chemical mechanical polishing slurries for enhanced polishing with minimal defects. Journal of The Electrochemical Society, 147(9), 3523–3528. https://doi.org/10.1149/1.1393931
  4. Evans, C. J., Paul, E., Dornfeld, D., Lucca, D. A., Byrne, G., Tricard, M., Klocke, F., Dambon, O., & Mullany, B. A. (2003). Material removal mechanisms in lapping and polishing. CIRP Annals, 52(2), 611–633. https://doi.org/10.1016/S0007-8506(07)60207-8
  5. International Organization for Standardization [ISO]. (2001). ISO 13317-1:2001, Determination of particle size distribution by gravitational liquid sedimentation methods — Part 1: General principles and guidelines.
  6. International Organization for Standardization [ISO]. (2007). ISO 8486-2:2007, Bonded abrasives — Determination and designation of grain size distribution — Part 2: Microgrits F230 to F2000.
  7. International Organization for Standardization [ISO]. (2020). ISO 13320:2020, Particle size analysis — Laser diffraction methods.
  8. Klocke, F. (2009). Manufacturing processes 2: Grinding, honing, lapping. Springer. https://doi.org/10.1007/978-3-540-92259-9
  9. Lee, T., Jeong, H., Lee, S., Kim, D., & Kim, H. (2020). Effect of the lapping platen groove density on the characteristics of microabrasive-based lapping. Micromachines, 11(8), 775. https://doi.org/10.3390/mi11080775
  10. Remsen, E. E., Anjur, S., Boldridge, D., Kamiti, M., Li, S., Johns, T., Dowell, C., Kasthurirangan, J., & Feeney, P. (2006). Analysis of large particle count in fumed silica slurries and its correlation with scratch defects generated by CMP. Journal of The Electrochemical Society, 153(5), G453–G461. https://doi.org/10.1149/1.2184036
  11. Trezona, R. I., Allsopp, D. N., & Hutchings, I. M. (1999). Transitions between two-body and three-body abrasive wear: Influence of test conditions in the microscale abrasive wear test. Wear, 225–229, 205–214. https://doi.org/10.1016/S0043-1648(98)00358-5
  12. Yin, T., Wang, Z., Doi, T., Kurokawa, S., Tan, Z., Ding, X., & Lin, H. (2021). Characteristic of SiC slurry in ultra precision lapping of sapphire substrates. International Journal of Precision Engineering and Manufacturing, 22(6), 1021–1029. https://doi.org/10.1007/s12541-021-00521-1

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.